Thickness Weight
Gauge Frac. Inch Dec. Inch mm oz/ft^2 lb/ft^2 kg/ft^2 kg/m^2 lb/m^2
0000000 1/2 .5 12.7 320 20.00 9.072 97.65 215.28
000000 15/32 .46875 11.90625 300 18.75 8.505 91.55 201.82
00000 7/16 .4375 11.1125 280 17.50 7.983 85.44 188.37
0000 13/32 .40625 10.31875 260 16.25 7.371 79.33 174.91
000 3/8 .375 9.525 240 15 6.804 73.24 161.46
00 11/32 .34375 8.73125 220 13.75 6.237 67.13 148.00
0 5/16 .3125 7.9375 200 12.50 5.67 61.03 134.55
1 9/32 .28125 7.14375 180 11.25 5.103 54.93 121.09
2 17/64 .265625 6.746875 170 10.625 4.819 51.88 114.37
3 1/4 .25 6.35 160 10 4.536 48.82 107.64
4 15/64 .234375 5.953125 150 9.375 4.252 45.77 100.91
5 7/32 .21875 5.55625 140 8.75 3.969 42.72 94.18
6 13/64 .203125 5.159375 130 8.125 3.685 39.67 87.45
7 3/16 .1875 4.7625 120 7.5 3.402 36.62 80.72
8 11/64 .171875 4.365625 110 6.875 3.118 33.57 74.00
9 5/32 .15625 3.96875 100 6.25 2.835 30.52 67.27
10 9/64 .140625 3.571875 90 5.625 2.552 27.46 60.55
11 1/8 .125 3.175 80 5 2.268 24.41 53.82
12 7/64 .109375 2.778125 70 4.375 1.984 21.36 47.09
13 3/32 .09375 2.38125 60 3.75 1.701 18.31 40.36
14 5/64 .078125 1.984375 50 3.125 1.417 15.26 33.64
15 9/128 .0703125 1.7859375 45 2.8125 1.276 13.73 30.27
16 1/16 .0625 1.5875 40 2.5 1.134 12.21 26.91
17 9/160 .05625 1.42875 36 2.25 1.021 10.99 24.22
18 1/20 .05 1.27 32 2 .9072 9.765 21.53
19 7/160 .04375 1.11125 28 1.75 .7938 8.544 18.84
20 3/80 .0375 .9525 24 1.50 .6804 7.324 16.15
21 11/320 .034375 .873125 22 1.375 .6237 6.713 14.80
22 1/32 .03125 .793750 20 1.25 .567 6.103 13.46
23 9/320 .028125 .714375 18 1.125 .5103 5.493 12.11
24 1/40 .025 .635 16 1 .4536 4.882 10.76
25 7/320 .021875 .555625 14 .875 .3969 4.272 9.42
26 3/160 .01875 .47625 12 .75 .3402 3.662 8.07
27 11/640 .0171875 .4365625 11 .6875 .3119 3.357 7.40
28 1/64 .015625 .396875 10 .625 .2835 3.052 6.73
29 9/640 .0140625 .3571875 9 .5625 .2551 2.746 6.05
30 1/80 .0125 .3175 8 .5 .2268 2.441 5.38
31 7/640 .0109375 .2778125 7 .4375 .1984 2.136 4.71
32 13/1280 .01015625 .25796875 6 1/2 .40625 .1843 1.983 4.37
33 3/320 .009375 .238125 6 .375 .1701 1.831 4.04
34 11/1280 .00859375 .21828125 5 1/2 .34375 .1559 1.678 3.70
35 5/640 .0078125 .1984375 5 .3125 .1417 1.526 3.36
36 9/1280 .00703125 .17859375 4 1/2 .28125 .1276 1.373 3.03
37 17/2560 .006640625 .168671875 4 1/4 .265625 .1205 1.297 2.87
38 1/160 .00625 .15875 4 .25 .1134 1.221 2.69
__________________


Stangnet
Shop Full Of Stuff.

Joey

Last edited by vipermanz; 07-25-2005 at 05:15 PM.
Reply With Quote
  #2  
Old 07-25-2005, 05:16 PM
vipermanz's Avatar
vipermanz vipermanz is offline
WeldingWeb Foreman
 
Join Date: Oct 2003
Location: Birmingham Al
Posts: 750
http://www4.law.cornell.edu/uscode/h...6----000-.html
__________________


Stangnet
Shop Full Of Stuff.

Joey
Reply With Quote
  #3  
Old 07-31-2005, 05:59 PM
atrain185 atrain185 is offline
WeldingWeb Apprentice
 
Join Date: Jul 2005
Location: ohio
Posts: 43
???

Just out of curiosity does anyone know what gauge aluminum foil is?
Reply With Quote
  #4  
Old 09-14-2005, 06:10 PM
ChuckD ChuckD is offline
Solderer
 
Join Date: Feb 2005
Location: Las Vegas
Posts: 9
atrain,
According to the Aluminum Association;
aluminum foil is considered "less than .006"
plate = 1/4" or more
sheet = .249" to .006"
foil = less than .006"
I just found this out last night, then I see this post today, so there you have it .
Reply With Quote
  #5  
Old 11-22-2005, 10:39 PM
atrain185 atrain185 is offline
WeldingWeb Apprentice
 
Join Date: Jul 2005
Location: ohio
Posts: 43
thanks chuck
Reply With Quote
  #6  
Old 04-16-2006, 02:00 AM
Bobcatter's Avatar
Bobcatter Bobcatter is offline
WeldingWeb Apprentice
 
Join Date: Apr 2006
Location: Florida
Posts: 41
Printable table in Word

Great information, thanks. I formatted it into Word so I could print and post it. Sheez, allergies, keep me up all night....

Okay, I made the file smaller, so I could upload it. You can put your own title on it.
Attached Files
File Type: doc ThicknessMetal.doc (101.5 KB, 3042 views)

Last edited by Bobcatter; 04-16-2006 at 02:10 AM.
Reply With Quote
  #7  
Old 07-19-2006, 02:29 PM
Arcie Arcie is offline
Solderer
 
Join Date: Jul 2006
Location: Washington State in the San Juan Islands
Posts: 8
Re: Printable table in Word

Thanks - for your efforts getting all the info to line up in "word". A real good refernce!
Reply With Quote
  #8  
Old 09-14-2008, 01:05 AM
wagin's Avatar
wagin wagin is offline
WeldingWeb Foreman
 
Join Date: Apr 2008
Location: Charlotte NC
Posts: 646
Re: Printable table in Word

Quote:
Originally Posted by Bobcatter View Post
Great information, thanks. I formatted it into Word so I could print and post it. Sheez, allergies, keep me up all night....

Okay, I made the file smaller, so I could upload it. You can put your own title on it.
thinks guy for the printable info. I had written down the common guages used and posted it on my tool box for purchasing info. This is more better. Thanks again.
__________________
Miller TrailBlazer 251
Miller HF-250-1
Miller MaxStar 150 STL
HyperTherm PowerMax 380 plasma
Lincoln PowerMig 180
Millermatic 252
Miller Diversion 180
Reply With Quote
  #9  
Old 07-22-2009, 10:32 AM
nctox's Avatar
nctox nctox is offline
WeldingWeb Journeyman
 
Join Date: Jul 2009
Location: Western NC
Posts: 141
Re: Printable table in Word

Quote:
Originally Posted by Bobcatter View Post
Great information, thanks. I formatted it into Word so I could print and post it. Sheez, allergies, keep me up all night....

Okay, I made the file smaller, so I could upload it. You can put your own title on it.
Thanks for the work. I made a few copies for the study, shop, etc...
__________________
Nctox,
Stickmate LX 235AC/160DC
HH210
Reply With Quote
  #10  
Old 07-22-2009, 11:50 AM
Magnetic Mechanic's Avatar
Magnetic Mechanic Magnetic Mechanic is offline
WeldingWeb Craftsman
 
Join Date: Jan 2008
Location: Arkansas
Posts: 1,202
Re: Sheet-Gauge Thickness Chart

Charts attached.
Attached Files
File Type: doc al weight.doc (106.5 KB, 168 views)
File Type: doc sm Gauge.doc (109.0 KB, 218 views)
File Type: doc sm weight.doc (99.5 KB, 137 views)
__________________
A butterfly without wings,
is just an ugly bug

Reply With Quote
  #11  
Old 08-05-2006, 10:45 PM
Lanmanb4's Avatar
Lanmanb4 Lanmanb4 is offline
WeldingWeb Journeyman
 
Join Date: Jun 2005
Location: Taberg, NY ( near Syracuse )
Posts: 137
Re: Sheet-Gauge Thickness Chart

Does anyone know what the gauge of typical car body metal is ?
Uhmmm particuliarly the older vehicles like a TR-8 ??
Reply With Quote
  #12  
Old 10-08-2006, 11:00 AM
fun4now.'s Avatar
fun4now. fun4now. is offline
WeldingWeb Craftsman
 
Join Date: Aug 2006
Location: near rochester NY
Posts: 1,195
Re: Sheet-Gauge Thickness Chart

newer cars can go to 26gage but most older are closer to 18.
thanks for the chart, verry helpfull.
__________________

summer is here, plant a tree for mother earth. if you dont have time or space, sponcer some one else to plant one for you.

feel free to shoot me a PM or e-mail me at [email]james@newyorkmetalart.com i got lots of time.
Reply With Quote
  #13  
Old 10-14-2006, 08:08 PM
metalman metalman is offline
WeldingWeb Journeyman
 
Join Date: Jan 2005
Location: Indiana
Posts: 61
Re: Sheet-Gauge Thickness Chart

Had to save that. Thanks for the chart!
Reply With Quote
  #14  
Old 10-14-2006, 11:13 PM
mla2ofus mla2ofus is offline
WeldingWeb Artisan
 
Join Date: Apr 2006
Location: Soda springs,Id
Posts: 2,270
Re: Sheet-Gauge Thickness Chart

My thanks to Vipermanz and Bobcatter for the chart. I printed off 2,one for my shop and one to make bets on how thick 10 ga is. Everyone i've ever talked about it w/ has always said it is 1/8", including myself!!!!
Thanks again,
Mike
__________________
Ol' Stonebreaker
"Experience is the name everyone gives to their mistakes"

Miller 175 mig
Miller thunderbolt ac/dc stick
Victor O/A setup
Makita chop saw
Reply With Quote
  #15  
Old 10-21-2006, 03:32 PM
codearc codearc is offline
WeldingWeb Apprentice
 
Join Date: Oct 2006
Posts: 48
Re: Sheet-Gauge Thickness Chart

i allways thought 10 gauge was 3.2mm thats what the old guys refer to in old money welding rods 12 gauge was 2.5
Reply With Quote
  #16  
Old 11-04-2006, 09:54 PM
bugdust bugdust is offline
WeldingWeb Journeyman
 
Join Date: Aug 2006
Location: Middleburg, FL USA
Posts: 72
Re: Sheet-Gauge Thickness Chart

I found this online at davesport.com

Grade and Description Chemistry Tensile Yield Rockwell Hardness
Units typical ksi ksi typical
1010
ERW tube C .08-.13
Mn .30-.60
P .035 max
S .035 max
45 32 RB55 min
1020
DOM tube C .15-.25
Mn .30-.60
P .040 max
S .050 max
80 70 RB80
4130
DOM tube
(chromoly) C .28-.33
Mn .40-.60
P .035
S .040
Si .15-.35
Cr .80-1.10
Mo .15-.25
100 90 RB90

As you can see, DOM tubing is nearly twice as strong in tension, and more than twice as strong in resistance to bending in comparison to the ERW tube. Also, the 4130 chromoly tube is only 20% stronger than standard DOM in tension.

Weights of typical tubing sizes

Outside Diameter Wall thickness Inside Diameter Type Weight, lbs/ft. Wgt/80ft.
1.25" 0.120 1.010" HREW/DOM 1.448 116
1.375" 0.120 1.135" HREW/DOM 1.608 128.6
1.5" 0.095" 1.310 HREW/DOM 1.426 114
1.5" 0.120" 1.260" HREW/DOM 1.769 141.5
1.75" 0.109" (FIA) 1.532" DOM 1.910 152.8
1.75" 0.120" 1.510" HREW/DOM 2.089 167.1



Gauge
Number
Thickness (Inches)
Pounds Per Sq. Ft.

Nominal
Tolerance Range

10
.1345
.1405 to .1285
5.48695

11
.1196
.1256 to .1136
4.87911

12
.1046
.1106 to .0986
4.26718

13
.0897
.0947 to .0847
3.65933

14
.0747
.0797 to .0697
3.04740

15
.0673
.0723 to .0623
2.74552

16
.0598
.0648 to .0548
2.43955

17
.0538
.0578 to .0498
2.19478

18
.0478
.0518 to .0438
1.95001

19
.0418
.0458 to .0378
1.70524

20
.0359
.0389 to .0329
1.46455

21
.0329
.0359 to .0299
1.34216

22
.0299
.0329 to .0269
1.21978

23
.0269
.0299 to .0239
1.09739

24
.0239
.0269 to .0209
.97501

25
.0209
.0239 to .0179
.85262

26
.0179
.0199 to .0159
.73023

27
.0164
.0184 to .0144
.66094
__________________
Always looking for another old VW, especially in the southeast.
Reply With Quote
  #17  
Old 11-05-2006, 11:51 PM
weldit weldit is offline
Solderer
 
Join Date: Dec 2004
Location: Saudi Arabia
Posts: 3
Re: Sheet-Gauge Thickness Chart

Thanks guys
Great infos
Reply With Quote
  #18  
Old 02-21-2007, 06:25 PM
zapster's Avatar
zapster zapster is offline
Moderator
 
Join Date: Jan 2006
Location: In A Nice Comfy Chair
Posts: 13,812
Re: Sheet-Gauge Thickness Chart

Quote:
Originally Posted by vipermanz
Thickness Weight
Gauge Frac. Inch Dec. Inch mm oz/ft^2 lb/ft^2 kg/ft^2 kg/m^2 lb/m^2
0000000 1/2 .5 12.7 320 20.00 9.072 97.65 215.28
000000 15/32 .46875 11.90625 300 18.75 8.505 91.55 201.82
00000 7/16 .4375 11.1125 280 17.50 7.983 85.44 188.37
0000 13/32 .40625 10.31875 260 16.25 7.371 79.33 174.91
000 3/8 .375 9.525 240 15 6.804 73.24 161.46
00 11/32 .34375 8.73125 220 13.75 6.237 67.13 148.00
0 5/16 .3125 7.9375 200 12.50 5.67 61.03 134.55
1 9/32 .28125 7.14375 180 11.25 5.103 54.93 121.09
2 17/64 .265625 6.746875 170 10.625 4.819 51.88 114.37
3 1/4 .25 6.35 160 10 4.536 48.82 107.64
4 15/64 .234375 5.953125 150 9.375 4.252 45.77 100.91
5 7/32 .21875 5.55625 140 8.75 3.969 42.72 94.18
6 13/64 .203125 5.159375 130 8.125 3.685 39.67 87.45
7 3/16 .1875 4.7625 120 7.5 3.402 36.62 80.72
8 11/64 .171875 4.365625 110 6.875 3.118 33.57 74.00
9 5/32 .15625 3.96875 100 6.25 2.835 30.52 67.27
10 9/64 .140625 3.571875 90 5.625 2.552 27.46 60.55
11 1/8 .125 3.175 80 5 2.268 24.41 53.82
12 7/64 .109375 2.778125 70 4.375 1.984 21.36 47.09
13 3/32 .09375 2.38125 60 3.75 1.701 18.31 40.36
14 5/64 .078125 1.984375 50 3.125 1.417 15.26 33.64
15 9/128 .0703125 1.7859375 45 2.8125 1.276 13.73 30.27
16 1/16 .0625 1.5875 40 2.5 1.134 12.21 26.91
17 9/160 .05625 1.42875 36 2.25 1.021 10.99 24.22
18 1/20 .05 1.27 32 2 .9072 9.765 21.53
19 7/160 .04375 1.11125 28 1.75 .7938 8.544 18.84
20 3/80 .0375 .9525 24 1.50 .6804 7.324 16.15
21 11/320 .034375 .873125 22 1.375 .6237 6.713 14.80
22 1/32 .03125 .793750 20 1.25 .567 6.103 13.46
23 9/320 .028125 .714375 18 1.125 .5103 5.493 12.11
24 1/40 .025 .635 16 1 .4536 4.882 10.76
25 7/320 .021875 .555625 14 .875 .3969 4.272 9.42
26 3/160 .01875 .47625 12 .75 .3402 3.662 8.07
27 11/640 .0171875 .4365625 11 .6875 .3119 3.357 7.40
28 1/64 .015625 .396875 10 .625 .2835 3.052 6.73
29 9/640 .0140625 .3571875 9 .5625 .2551 2.746 6.05
30 1/80 .0125 .3175 8 .5 .2268 2.441 5.38
31 7/640 .0109375 .2778125 7 .4375 .1984 2.136 4.71
32 13/1280 .01015625 .25796875 6 1/2 .40625 .1843 1.983 4.37
33 3/320 .009375 .238125 6 .375 .1701 1.831 4.04
34 11/1280 .00859375 .21828125 5 1/2 .34375 .1559 1.678 3.70
35 5/640 .0078125 .1984375 5 .3125 .1417 1.526 3.36
36 9/1280 .00703125 .17859375 4 1/2 .28125 .1276 1.373 3.03
37 17/2560 .006640625 .168671875 4 1/4 .265625 .1205 1.297 2.87
38 1/160 .00625 .15875 4 .25 .1134 1.221 2.69


Chart..
Check out 23 guage..

...zap!
__________________


I am not completely insane..
Some parts are missing

I have figured out that keeping everyone happy is nearly impossible but pissing people off is easy and fun.
Reply With Quote
  #19  
Old 08-27-2007, 08:11 PM
BWS29128 BWS29128 is offline
WeldingWeb Apprentice
 
Join Date: Aug 2007
Posts: 46
Re: Sheet-Gauge Thickness Chart

Can someone PLEASE explain to me why I didn't find this message board until last week, when I really needed all this info 3 weeks ago???



Hee Hee
Reply With Quote
  #20  
Old 01-19-2008, 10:49 PM
smokeshow smokeshow is offline
WeldingWeb Tradesman
 
Join Date: Oct 2007
Posts: 249
Re: Sheet-Gauge Thickness Chart

Great info...

Saving most of it...
Reply With Quote
  #21  
Old 01-20-2008, 11:48 AM
fun4now.'s Avatar
fun4now. fun4now. is offline
WeldingWeb Craftsman
 
Join Date: Aug 2006
Location: near rochester NY
Posts: 1,195
Re: Sheet-Gauge Thickness Chart

well at first glance one would think this is very helpful. BUT all it really dose if confuse you even more ???
none of the #'s match ???what chart do we trust ??

vipermanz...............VS................bugdust

COLOR="blue"]vipermanz[/color]...............
20 3/80 .0375
27 11/640 .0171875
15 9/128 .0703125

VS................bugdust

20 .0359
27 .0164
15 .0673


at first i just thought it was a simple question of rounding it up to keep the # from going on forever, but???? 20 gage .0375 and 20 gage .0359 are way to far to be rounding for simplicity sake ?? so what gives ?? must be a tolerance thing ??
the only solution i see is ....
__________________

summer is here, plant a tree for mother earth. if you dont have time or space, sponcer some one else to plant one for you.

feel free to shoot me a PM or e-mail me at [email]james@newyorkmetalart.com i got lots of time.
Reply With Quote
  #22  
Old 01-31-2008, 12:23 PM
Magnetic Mechanic's Avatar
Magnetic Mechanic Magnetic Mechanic is offline
WeldingWeb Craftsman
 
Join Date: Jan 2008
Location: Arkansas
Posts: 1,202
Re: Sheet-Gauge Thickness Chart

Name:  chart.jpg
Views: 15651
Size:  117.4 KB
blow this up 2x to read it

Last edited by Magnetic Mechanic; 01-31-2008 at 12:29 PM. Reason: no explanation
Reply With Quote
  #23  
Old 02-03-2008, 07:30 PM
ddog's Avatar
ddog ddog is offline
WeldingWeb Journeyman
 
Join Date: Jan 2008
Location: Port Jervis, NY
Posts: 196
Re: Sheet-Gauge Thickness Chart

very helpful!!!!! printed a copy for the tool box... Thanks everyone
Reply With Quote
  #24  
Old 08-04-2008, 05:45 PM
davidmn davidmn is offline
Solderer
 
Join Date: Aug 2008
Posts: 1
I was to hasty in my previous reply.

In the start window I get the button 'Try It' which I clicked. But it still ends after 10 minutes.
Reply With Quote
  #25  
Old 08-13-2008, 12:43 AM
cranest cranest is offline
WeldingWeb Journeyman
 
Join Date: Dec 2007
Location: Reno, NV
Posts: 61
Re: Sheet-Gauge Thickness Chart

Just to point out ferrous metal sheet and aluminum sheet gauge numbers refer to different thicknesses, meaning 10 ga. steel sheet is different thickness that 10 ga aluminum sheet. Though there are several good sources on the web, I like Aircraft Spruce and Specialty's info sheets out of their online catalog. The catalog is worth having just for the info, just like the old Starrett catalogs, verituble encyclopedias of measuring and setup info. Try this page:
http://www.aircraftspruce.com/catalo...metalinfo1.php
Reply With Quote
Reply

Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off

Forum Jump


All times are GMT -4. The time now is 02:59 AM.


Powered by vBulletin® Version 3.8.7
Copyright ©2000 - 2013, vBulletin Solutions, Inc.
Copyright ©2000 - 2013, Penton Media, Inc. All rights reserved.