can ya fix me tractor bit

had a bloke come in to day need a manifold for is tractor patch up till he can find another one
it was in a sad way bits disappeared when I was grinding it so I had alot of building up to do in the end it turned out ok the build up weld isn't the pretty but didn't need to seen it was getting sanded to shape this should keep him going
Name:  MVC-001S.JPG
Views: 854
Size:  36.9 KB
before
Name:  MVC-002S.JPG
Views: 853
Size:  29.4 KB
inbetween
Name:  MVC-005S.JPG
Views: 853
Size:  32.6 KB
after lots of build
Name:  MVC-006S.JPG
Views: 854
Size:  29.5 KB
done
Name:  MVC-008S.JPG
Views: 854
Size:  33.9 KB
__________________
Creative metal


A married man should forget his mistakes. There's no use in two people remembering the same thing!
Reply With Quote
  #2  
Old 03-06-2007, 05:19 AM
chopper5 chopper5 is offline
WeldingWeb Craftsman
 
Join Date: Nov 2005
Location: utcia michigan
Posts: 1,277
Re: can ya fix me tractor bit

now just repaint it and it will look new, good job
__________________

Chuck
ASME Pressure Vessel welder
Reply With Quote
  #3  
Old 03-06-2007, 06:23 AM
David R's Avatar
David R David R is offline
Master Welder
 
Join Date: Feb 2007
Location: West By Golly Shelby NY
Posts: 7,246
Re: can ya fix me tractor bit

Quite the job!

David
__________________
Real world weldin.

When I grow up I want to be a tig weldor.
Reply With Quote
  #4  
Old 03-06-2007, 08:09 AM
ChenS ChenS is offline
WeldingWeb Apprentice
 
Join Date: May 2006
Posts: 36
Re: can ya fix me tractor bit

very nice!
__________________
Idealarc 300\300 TIG AC\DC
Reply With Quote
  #5  
Old 03-06-2007, 08:49 AM
fun4now.'s Avatar
fun4now. fun4now. is offline
WeldingWeb Craftsman
 
Join Date: Aug 2006
Location: near rochester NY
Posts: 1,195
Re: can ya fix me tractor bit

now i bet he stops looking for a new one, after all with a fix like that he will likely bring you the other side.LOL
thats a lot of build up for TIG, was it TIG ?? the one on the right looks like tig but hard to tell on the big one up front.
__________________

summer is here, plant a tree for mother earth. if you dont have time or space, sponcer some one else to plant one for you.

feel free to shoot me a PM or e-mail me at [email]james@newyorkmetalart.com i got lots of time.
Reply With Quote
  #6  
Old 03-06-2007, 02:34 PM
wello's Avatar
wello wello is offline
Moderator
 
Join Date: May 2006
Location: Wellington Austraila
Posts: 922
Re: can ya fix me tractor bit

yeah it was done with the tig fun4now took about 2 1/2 hours to do all 3 outlets and weld the fitting on
__________________
Creative metal


A married man should forget his mistakes. There's no use in two people remembering the same thing!
Reply With Quote
  #7  
Old 03-06-2007, 04:43 PM
lorenzo's Avatar
lorenzo lorenzo is offline
WeldingWeb Foreman
 
Join Date: Dec 2006
Location: Southern New Hampshire
Posts: 919
Re: can ya fix me tractor bit

Good job.... Hope he appreciates your efforts. did you have to re-shape the exhaust ports as well?
__________________
_________________
Chris
Reply With Quote
  #8  
Old 03-06-2007, 07:20 PM
David R's Avatar
David R David R is offline
Master Welder
 
Join Date: Feb 2007
Location: West By Golly Shelby NY
Posts: 7,246
Re: can ya fix me tractor bit

Quote:
Originally Posted by lorenzo
Good job.... Hope he appreciates your efforts. did you have to re-shape the exhaust ports as well?
I think its a water manifold.

David
__________________
Real world weldin.

When I grow up I want to be a tig weldor.
Reply With Quote
  #9  
Old 03-07-2007, 01:51 AM
wello's Avatar
wello wello is offline
Moderator
 
Join Date: May 2006
Location: Wellington Austraila
Posts: 922
Re: can ya fix me tractor bit

Quote:
Originally Posted by David R
I think its a water manifold.

David
yep it is a water manifold
__________________
Creative metal


A married man should forget his mistakes. There's no use in two people remembering the same thing!
Reply With Quote
  #10  
Old 03-07-2007, 05:19 AM
lorenzo's Avatar
lorenzo lorenzo is offline
WeldingWeb Foreman
 
Join Date: Dec 2006
Location: Southern New Hampshire
Posts: 919
Re: can ya fix me tractor bit

Quote:
Originally Posted by wello
yep it is a water manifold
Sorry my bad...........
__________________
_________________
Chris
Reply With Quote
  #11  
Old 03-07-2007, 01:38 PM
Doolittle Doolittle is offline
WeldingWeb Craftsman
 
Join Date: Sep 2006
Posts: 1,052
Re: can ya fix me tractor bit

wello, did those just corrode to peices like that? wow.
__________________
Various Grinders
Victor Journeyman torch
200cf Acet. 250cf oxygen
Lincoln 175 plus/alpha2 gun
Lincoln v205t tig
Lincoln 350mp
Esab 650 plasma
When you can get up in the morning, Its a good day.
Live each day like its your last.
Reply With Quote
  #12  
Old 03-07-2007, 10:35 PM
ZTFab's Avatar
ZTFab ZTFab is online now
WeldingWeb Artisan
 
Join Date: Aug 2006
Location: San Dimas, CA
Posts: 2,247
Re: can ya fix me tractor bit

Nice job Wello.



- Paul
__________________
Hold my beer...watch this.
Reply With Quote
Reply

Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off

Forum Jump


All times are GMT -4. The time now is 11:19 PM.


Powered by vBulletin® Version 3.8.7
Copyright ©2000 - 2013, vBulletin Solutions, Inc.
Copyright ©2000 - 2013, Penton Media, Inc. All rights reserved.