    Trying to find an answer on this.

    Do laser cut holes experience the same work hardening seen with plasma cut holes?

    I am looking to outsource one of my products and need to decide if I have them cut the holes to pre-tap size.

    I know on plasma cut holes that would be suicide, plasma cut is also not round enough but drilling a plasma cut pilot is usually difficult in itself.
    www.FirehouseFabricators.com

    [B]

    Lincoln 210mp
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  2. #2
    Join Date
    Mar 2017
    Location
    Forest Grove OR
    Posts
    274
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by BrooklynBravest View Post
    Hey guys,

    Trying to find an answer on this.

    Do laser cut holes experience the same work hardening seen with plasma cut holes?

    I am looking to outsource one of my products and need to decide if I have them cut the holes to pre-tap size.

    I know on plasma cut holes that would be suicide, plasma cut is also not round enough but drilling a plasma cut pilot is usually difficult in itself.
    I read up on the idea out of curiosity just now, it seems to be the air used to evacuate the molten metal. Nitrogen in the air causes nitrite hardening in the surface. Thus it wouldn't matter if it were optical power or electrical power that melted the steel, it's the high nitrogen content air stream that hardens it. A solution was offered in industircal CNC cutters that use pure oxygen, this hardnign does not happen, but you can't convert an "air" system to an O2 system, it has to be designed for it.

    A work around offered was using a carbide deburring bit to cut off the hardened surface which is only about .006" to .010" thick.
    Everlast 350 EXT - Thermal Dynamics Cutmaster 52 - Rogue Fabrication M600 xHD tube bender
    Milwaukee 4208 Mag Drill - Shopmaster Eldorado Combo mill/lathe machine with DRO.

  3. #3
    Join Date
    Oct 2013
    Location
    Long Island, NY
    Posts
    2,154
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by Chad86tsi View Post
    I read up on the idea out of curiosity just now, it seems to be the air used to evacuate the molten metal. Nitrogen in the air causes nitrite hardening in the surface. Thus it wouldn't matter if it were optical power or electrical power that melted the steel, it's the high nitrogen content air stream that hardens it. A solution was offered in industircal CNC cutters that use pure oxygen, this hardnign does not happen, but you can't convert an "air" system to an O2 system, it has to be designed for it.

    A work around offered was using a carbide deburring bit to cut off the hardened surface which is only about .006" to .010" thick.
    It just dawned on me when i have this company laser cut tubing for me, and I countersink (heavily) one of the holes and never have an issue.

    When i try that with a plasma cut hole it murders a $40 countersink.
    www.FirehouseFabricators.com

    [B]

    Lincoln 210mp
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  4. #4
    Join Date
    Apr 2015
    Location
    Fredericksburg, VA
    Posts
    2,187
    Post Thanks / Like

    Re: Tapping laser cut holes?

    I do not use them, but would a reamer be a good idea? Have them laser cut to a certain size then pass a reamer through it. If so, that would be a quick operation in your new drill.
    Here is some info form the web


    FINAL HOLE
    REAMER SIZE Reduce Drill Hole Size Reduce Drill Hole
    By (mm) Size By (inch)

    mm inch MIN MAX MIN MAX
    0.20mm .00787" -0.04mm -0.06mm -0.00157" -0.00236"
    0.30mm .01181" -0.05mm -0.08mm -0.00197" -0.00315"
    0.40mm .01575" -0.05mm -0.10mm -0.00197" -0.00394"
    0.50mm .01969" -0.05mm -0.12mm -0.00197" -0.00472"
    0.60mm .02362" -0.05mm -0.12mm -0.00197" -0.00472"
    2.00mm .07874" -0.05mm -0.12mm -0.00197" -0.00472"
    6.00mm .23622" -0.15mm -0.20mm -0.00591" -0.00787"
    10.00mm .39370" -0.15mm -0.20mm -0.00591" -0.00787"
    15.00mm .59055" -0.30mm -0.40mm -0.01181" -0.01575"
    20.00mm .78740" -0.30mm -0.40mm -0.01181" -0.01575"
    25.00mm .98425" -0.30mm -0.50mm -0.01181" -0.01969
    Millermatic 252 MIG
    Miller Dynasty 200DX TIG
    Miller Spectrum 625 Plasma
    Altas 12x36 Metal Lathe
    Bridgeport Milling Machine
    www.psacustomcreations.com

  5. #5
    Join Date
    Mar 2017
    Location
    Forest Grove OR
    Posts
    274
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by BrooklynBravest View Post
    It just dawned on me when i have this company laser cut tubing for me, and I countersink (heavily) one of the holes and never have an issue.

    When i try that with a plasma cut hole it murders a $40 countersink.
    I'm glad you brought it up, I was unaware of this prior. Saves me trouble in the future

    Another idea I saw offered was just a pierce to create a center punch like hole locator for drilling later. You get the precision location but it wont' murder your bits.
    Everlast 350 EXT - Thermal Dynamics Cutmaster 52 - Rogue Fabrication M600 xHD tube bender
    Milwaukee 4208 Mag Drill - Shopmaster Eldorado Combo mill/lathe machine with DRO.

  6. Likes Dee_veloper liked this post
  7. #6
    Join Date
    Oct 2013
    Location
    NOVA
    Posts
    353
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Need to be careful with laser cut and plasma. I had some plates recently where we had the vendor laser cut some pilot holes for us in 1/4" plate to drill and tap out to #8-32. We went through 10 of the #29 bits on the first 30 plates with 4 holes per plate and really good bits.

    Had to switch to carbide bits on the mill to make it work. Almost defeated the purpose of the pilot holes.

    Sent from my SM-N950U using Tapatalk
    Multimatic 200
    Ellis 1800
    Haberle S225 9" cold saw
    MM 300; Spoolmate 30A w/ WC-24
    TB 302G
    Dynasty 280 DX Tigrunner

  8. #7
    Join Date
    Dec 2018
    Posts
    2,752
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Dunno why anyone would want to have some laser cut stuff to tap. Be like throwing darts at a wall.

    Hole diameters for tapping are pretty precise, depending on length of thread engagement. Bigger hole for deeper thread. I mean, you're talkin' thousands difference. Drill size is generally +- one letter,, number, or fractional size according to depth, and class of fit.

    I can't imagine any hot cutting process would be that accurate

  9. #8
    Join Date
    Dec 2018
    Posts
    2,752
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by Drooopy View Post
    Need to be careful with laser cut and plasma. I had some plates recently where we had the vendor laser cut some pilot holes for us in 1/4" plate to drill and tap out to #8-32. We went through 10 of the #29 bits on the first 30 plates with 4 holes per plate and really good bits.

    Had to switch to carbide bits on the mill to make it work. Almost defeated the purpose of the pilot holes.

    Sent from my SM-N950U using Tapatalk
    Yeah, that was what I was sayin'. Better to just drill the things, and tap them.

    Pilot hole for small holes would be hard to work with anyway, seems that you'd tear up the bits in short order, what with them catching the edge of the hole with the outside edge of the drill cutting edge

  10. #9
    Join Date
    Jan 2005
    Posts
    4,104
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by Chad86tsi View Post
    I'm glad you brought it up, I was unaware of this prior. Saves me trouble in the future

    Another idea I saw offered was just a pierce to create a center punch like hole locator for drilling later. You get the precision location but it wont' murder your bits.
    I would use a divot mark for locating centers, instead of piercing all the way through the plate..
    Esab/Lorch ET-220i
    Esab 160i caddy
    Thermal LM-200 Lincoln feeders
    Thermal Pee-Wee 85s
    2-Thermal 60i- 3phase /RPC powered (Beast)
    Thermal Drag-gun 35C
    INE 1500
    Klutch 80i +

  11. Likes ronsii liked this post
  12. #10
    Join Date
    Dec 2003
    Location
    Fairfield,CT
    Posts
    1,369
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by Brand X View Post
    I would use a divot mark for locating centers, instead of piercing all the way through the plate..
    This^^^. I have done this in sheetcam. My drawing just has a "period" where I want to make the hole. I have done it a couple of times. Little tricky in the beginning to set it up. Also Acourtjester gave me a good idea to lower the voltage when making the peck operation so it just makes a divot.
    www.tjsperformance.com
    Dynasty 300 DX
    HTP 240
    HTP Microcut 380
    Hyperthem 85
    JD2 Hyd Bender and HF Hyd Ring Roller all in one =(Frankenbender)
    Bpt. Mill/DRO
    4' x 8' CNC Plasma Table
    Instagram: tjsperformance
    YT: TJS Welding and Fabrication

  13. #11
    Join Date
    Oct 2013
    Location
    Long Island, NY
    Posts
    2,154
    Post Thanks / Like

    Re: Tapping laser cut holes?

    To follow up on this, I did have the parts cut. Aprox $3000 worth. So... We'll see if it works. Worst I go back to plan A and weld a nut on the back for this batch no harm done and pilot hole the next ones to be drilled and then tapped.
    www.FirehouseFabricators.com

    [B]

    Lincoln 210mp
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  14. #12
    Join Date
    Mar 2010
    Location
    Connecticut
    Posts
    40
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Not really going to help you out now, but if you have more to do, I've had really good luck tapping holes that have been water jet cut. About the only negative versus a drilled hole is the hole tends to have a bit of a draft angle especially on thicker plates.

  15. #13
    Join Date
    May 2012
    Location
    Ontario, Canada
    Posts
    1,322
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Talk to who does your laser cutting.

    The new laser, waterjet cutters can have drill heads mounted so they can drill holes.
    Especially on waterjets, it helps to pierce with the drill.

  16. #14
    Join Date
    Oct 2007
    Location
    New Hampshire, North Carolina
    Posts
    3,336
    Post Thanks / Like

    Re: Tapping laser cut holes?

    The hardening on plasma (and laser) cut holes that will inhibit tapping is caused when using compressed air as the plasma gas or assist gas (laser). Air is 80% nitrogen, and the heat of the process combined with nitrogen creates a "case" hardened nitrided edge, much too hard to tap without destroying the tap.

    The fix? For plasma cutting you just need the right system! High Definition class plasma cutters (Hypertherm's XPR series plasma cutters) use oxygen as the plasma gas and oxygen as the shield (the patented "TrueHole" process) for eliminating the taper, the start divot and the stop ding as well as to remove the nitride hardening on plasma cut holes from3/16" to about 1" in diameter. The CNC machines that are equipped with HPR plasma must be of high precision (will not work on the same machines that typically use air plasma) and specifically designed for XPR plasma systems. These plasma tables with TrueHole start at about $120k (far less costly than a laser rated for the same thickness range). Jim Colt

  17. Likes ronsii liked this post
  18. #15
    Join Date
    Oct 2013
    Location
    Long Island, NY
    Posts
    2,154
    Post Thanks / Like

    Re: Tapping laser cut holes?

    Quote Originally Posted by jimcolt View Post
    The hardening on plasma (and laser) cut holes that will inhibit tapping is caused when using compressed air as the plasma gas or assist gas (laser). Air is 80% nitrogen, and the heat of the process combined with nitrogen creates a "case" hardened nitrided edge, much too hard to tap without destroying the tap.

    The fix? For plasma cutting you just need the right system! High Definition class plasma cutters (Hypertherm's XPR series plasma cutters) use oxygen as the plasma gas and oxygen as the shield (the patented "TrueHole" process) for eliminating the taper, the start divot and the stop ding as well as to remove the nitride hardening on plasma cut holes from3/16" to about 1" in diameter. The CNC machines that are equipped with HPR plasma must be of high precision (will not work on the same machines that typically use air plasma) and specifically designed for XPR plasma systems. These plasma tables with TrueHole start at about $120k (far less costly than a laser rated for the same thickness range). Jim Colt
    Im gonna start saving now... lol.



    For anyone wondering, the parts came (900 lbs worth) and I was able to tap them no problem with gun taps and a tapping head. Worked flawlessly.
    www.FirehouseFabricators.com

    [B]

    Lincoln 210mp
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  19. Likes thegary liked this post

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,594,871,023.53211 seconds with 14 queries