    So I got the MigMax and I gave it a whirl last night. Had a few questions.

    - My test steel is 1/8th inch steel from Home Depot. When I look at the manual settings it recommends E4 manual setting for 220V and 0.30 wire.

    Why is the auto setting for 1/8th inch so much higher in terms of voltage? The welds I tried in manual seemed too cold and the ones in auto seemed too hot. Can’t make sense of it.

    - When in auto setting do I set the wire speed at all or is that bypassed?

    HFs manuals are not for the uninitiated


    Sent from my iPhone using Tapatalk

  2. #2
    Join Date
    Jun 2012
    Location
    CT
    Posts
    6,501
    Post Thanks / Like

    Re: Questions about my new MigMax 215

    In the auto mode, ignore your wire speed dial (it is all bypassed). If the welds are too hot, adjust the left knob down to get less heat input. In manual mode, wire speed represents your amps/heat input, voltage controls the weld bead profile (tall, ropey, convex on one end of the spectrum, flat or concave on the other end of the spectrum.). This video will help you set your machine in manual mode.

    Miller Multimatic 255

  3. Likes kyngfish liked this post
  4. #3
    Join Date
    Aug 2020
    Posts
    10
    Post Thanks / Like

    Re: Questions about my new MigMax 215

    Thanks!

    One more question. As the metal gets hotter do I need to turn the voltage down - if I’m welding the same piece for a longer time


    Sent from my iPhone using Tapatalk

  5. #4
    Join Date
    Jun 2012
    Location
    CT
    Posts
    6,501
    Post Thanks / Like

    Re: Questions about my new MigMax 215

    Potentially yes. Well either voltage or more likely wire feed speed. But unless you are welding a small piece of metal, that isn't too likely.
    Miller Multimatic 255

  6. #5
    Join Date
    Aug 2020
    Posts
    10
    Post Thanks / Like

    Re: Questions about my new MigMax 215

    Test welds. So yeah.


    Sent from my iPhone using Tapatalk

  7. #6
    Join Date
    Jun 2012
    Location
    CT
    Posts
    6,501
    Post Thanks / Like

    Re: Questions about my new MigMax 215

    If you are just practicing on coupons, you could always put them in a bucket of water to quench them. Not a normally recommended practice but for test coupons it won't hurt anything. That way you don't need to keep fiddling with your settings. I dunk them every 2-3 beads.
    Miller Multimatic 255

  8. Likes Broccoli1 liked this post
  9. #7
    Join Date
    Dec 2007
    Location
    Los Angeles
    Posts
    8,879
    Post Thanks / Like

    Re: Questions about my new MigMax 215

    You really wont need to adjust the settings during welding as you would/should not be making such a long weld.

    On a real project you will make it a banana in a second if you don't move around the piece.

    https://m.lincolnelectric.com/es-es/...on-detail.aspx



    When I was learning I just moved on to a separate test piece and let the first one cool down.
    Ed Conley
    http://www.screamingbroccoli.com/
    MM252
    MM211 (Sold)
    Passport Plus & Spool gun
    Lincoln SP135 Plus- (Gone to a good home)
    Klutch 120v Plasma cutter
    SO 2020 bender
    Beer in the fridge

  10. Likes wmgeorge liked this post
+ Reply to Thread

Quick Reply Quick Reply

Register Now

Please enter the name by which you would like to log-in and be known on this site.

Please enter a password for your user account. Note that passwords are case-sensitive.

Please enter a valid email address for yourself.

A) Welding/Fabrication Shop
B) Plant/Production Line
C) Infrastructure/Construction/Repair or Maintenance/Field Work
D) Distributor of Welding Supplies or Gases
E) College/School/University
F) Work Out of Home

A) Corporate Executive/Management
B) Operations Management
C) Engineering Management
D) Educator/Student
E) Retired
F) Hobbyist

Log-in