    In the process of moving my DoAll saw we put too much force on the table and broke the cast iron table bracket. When we inspected the bracket we could see that it was repaired by brazing in the past. The first picture shows the saw with the table askew due to the broken bracket.

    1. DoAll Saw
    Name:  1. DoAll Saw.jpg
Views: 536
Size:  45.5 KB

    If you look carefully at the following picture you can see the new crack next to the old repair.

    2. Crack and previous repair
    Name:  2. Crack and previous repair.jpg
Views: 540
Size:  108.8 KB

    For the next two pictures I have removed half of the casting, so that you can see the cracked face as well as the previous repair.

    3. Cracked face
    Name:  3. Cracked face.jpg
Views: 536
Size:  116.9 KB

    4. Cracked face and previous repair
    Name:  4. Cracked face and previous repair.jpg
Views: 535
Size:  104.1 KB

    The first step was to vee out the crack.

    5. Crack veed out
    Name:  5. Crack veed out.jpg
Views: 536
Size:  132.9 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  2. Likes ronsii liked this post
  3. #2
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    292
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    I mounted the bracket in the table to hold all of the pieces in the correct orientation.

    6. Bracket in place for brazing
    Name:  6. Bracket in place for brazing.jpg
Views: 531
Size:  117.7 KB

    My friend John used one of my Oxyacetylene torches to preheat the casting to 900° F.

    7. Preheating with one torch
    Name:  7. Preheating with one torch.jpg
Views: 527
Size:  112.3 KB

    I used a second Oxyacetylene torch to braze the joint. I used the Lincoln pre-coated brazing rods that I picked up from Lowes. I like the pre-coated rods because it avoids stopping the brazing process to continually dip the rods into the flux can.

    8. Crack brazed
    Name:  8. Crack brazed .jpg
Views: 533
Size:  81.9 KB

    I covered the brazed joint with kitty litter and let it cool off overnight.

    9. Cover area with Kitty litter to cool slowly
    Name:  9. Cover area with Kitty litter to cool slowly.jpg
Views: 531
Size:  107.3 KB

    I used a brass wire wheel to clean up the joint. Here are three pictures of the brazed joint cleaned up.

    10. Inside of brazed joint
    Name:  10. Inside of brazed joint.jpg
Views: 534
Size:  96.3 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  4. Likes ronsii liked this post
  5. #3
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    292
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    11. Outside of brazed joint
    Name:  11. Outside of brazed joint.jpg
Views: 533
Size:  109.7 KB

    12. Entire bracket repaired
    Name:  12. Entire bracket repaired.jpg
Views: 539
Size:  178.2 KB

    I decided to paint the saw. The first step was to Dual Action sand the saw to blend the paint chips. I didn't bother to use primer surfacer to make the surface completely flat.

    13. Saw DA sanded
    Name:  13. Saw DA sanded.jpg
Views: 533
Size:  86.7 KB

    Here is a picture of the saw before painting for comparison

    14. Saw before painting
    Name:  14. Saw before painting.jpg
Views: 530
Size:  82.4 KB

    Here is a picture of the saw after I primed it.

    15. Saw primed
    Name:  15. Saw primed.jpg
Views: 533
Size:  71.5 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  6. Likes ronsii, JJW liked this post
  7. #4
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    292
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Here is a picture of the saw painted.

    16. Saw painted
    Name:  16. Saw painted.jpg
Views: 532
Size:  81.2 KB

    My friend John was in a GM plant downriver and noticed them scrapping a similar saw that was caught in a flood. He asked them to send him the selection dial for my saw, which the did. I don't typically use the selection dial, but it dresses up the saw.

    17. Close up of Job selector dial
    Name:  17. Close up of Job selector dial.jpg
Views: 530
Size:  77.3 KB

    This saw was built in the 40's so it is older than I. It still works fine including the blade welder, but it can only weld carbon steel blades not bi-metal.

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  8. #5
    Join Date
    Jun 2012
    Location
    Sebeka and Bemidji MN
    Posts
    14,554
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Looks like an excellent repair

    Saw looks great! I like the additional side piece - looks really nice there.

    I haven't learned to oxy braze yet, just tig brazing so far.
    Dave J.

    Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~

    Airco 300 - Syncro 350
    Invertec v250-s
    Thermal Arc 161 and 300
    MM210
    Dialarc
    Tried being normal once, didn't take....I think it was a Tuesday.

  9. Likes ronsii liked this post
  10. #6
    Join Date
    Dec 2016
    Posts
    111
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Looks good


    Sent from my iPhone using Tapatalk

  11. #7
    Join Date
    Mar 2007
    Location
    MidWest
    Posts
    526
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Good on you for resurrecting old iron. Looks good, wish I could braze like that.
    Geezer
    Power Mig 255C
    185 TIG
    Blue 175 MIG
    Ranger 8 Kohler 20HP
    1974 5K Lincoln/Wisconsin Powered (Cherry)
    Victor/Harris O/A
    K 487 Spool Gun

  12. #8
    Join Date
    Dec 2018
    Posts
    3,185
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    That is a beautiful job.

  13. #9
    Join Date
    May 2017
    Location
    Pitman PA
    Posts
    476
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Thats some nice lookin work right there...good to save old stuff it seen a lot of work in its day and looks like it will see a lot more...older stuff works better most of the time and is simpler and easier to use anyway

  14. Likes ronsii liked this post
  15. #10
    Join Date
    Oct 2016
    Location
    Delavan WI
    Posts
    493
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Quote Originally Posted by Popeye an old miner View Post
    .older stuff works better most of the time and is simpler and easier to use anyway
    Truer words may never have been spoken before.
    Old stuff rocks!

  16. Likes ronsii liked this post
  17. #11
    Join Date
    Feb 2015
    Location
    Texas
    Posts
    187
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Good looking repair and shop. Should last another 80 years at least
    Miller 350 Dynasty
    Miller Trailblazer
    Miller 625 Plasma

    Lincoln Power MIG
    Victor oxy/acetylene
    Hyperthem 85

  18. Likes ronsii liked this post
  19. #12
    Join Date
    Jul 2016
    Location
    Midwest
    Posts
    405
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    I Love repairs like this. Nice work !.
    Thermal Arc 320SP ( Lorch )
    Cobra Pythons
    Thermal Arc 300 AC/DC ( Sanrex )
    ESAB 301i AC/DC ( Lorch )
    Thermal Arc 161STL ( WTL )
    Thermal Arc 190S ( Sanrex )
    Cut Master 82, 42. Cut45 ( WTL )
    Victor Gas Apps.
    Boxes and boxes of welding crap.

  20. #13
    Join Date
    Mar 2005
    Location
    Under a Rock
    Posts
    5,489
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Job selector dial makes all the difference..... Looks great.
    Miller 211
    Hypertherm PM 45
    1961 Lincoln Idealarc 250
    HTP 221


    True Wisdom only comes from Pain.

  21. #14
    Join Date
    Nov 2006
    Location
    near Rochester NY
    Posts
    69
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Don, you should give it a try with welding bi-metal blades. The toolroom where I used to work had WWWII tagged DoAll bandsaws! We would weld both high carbon & Bi-Metal blades on them. Great job on the saw!

  22. #15
    Join Date
    Apr 2014
    Location
    MN/WI
    Posts
    342
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    If they were scrapping the same saw, did you try to get the table arm off it? Just in case yours gets broken again?
    Century buzzbox that I learned on 40+ years ago (was Dad's)
    Crappy Century 110volt mig 70 amp pigeon pooper.
    Lincoln Idealarc TIG-300

  23. #16
    Join Date
    Oct 2014
    Posts
    2,621
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    I'd guess the original repair wasn't heated and/or slow cooled enough because the new crack appeared right next to the braze.

  24. #17
    Join Date
    Dec 2018
    Posts
    3,185
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Maybe he shoulda G'mawed it

  25. #18
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    292
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Quote Originally Posted by MinnesotaDave View Post
    Looks like an excellent repair
    Saw looks great! I like the additional side piece - looks really nice there.
    I haven't learned to oxy braze yet, just tig brazing so far.
    I agree that the job selector makes the saw look complete.

    Quote Originally Posted by ljmelius View Post
    Looks good
    Thanks

    Quote Originally Posted by Popeye an old miner View Post
    Thats some nice lookin work right there...good to save old stuff it seen a lot of work in its day and looks like it will see a lot more...older stuff works better most of the time and is simpler and easier to use anyway
    I like old stuff as well. When I got rid of my Putnam 1890 lathe I found a good home for it.

    1. Old 1890 Putnam Lathe
    Name:  1. Old 1890 Putnam Lathe.jpg
Views: 219
Size:  71.8 KB

    Quote Originally Posted by BluCllrPlt View Post
    Good looking repair and shop. Should last another 80 years at least
    Or at least it will outlast me.

    Quote Originally Posted by geezer View Post
    Good on you for resurrecting old iron. Looks good, wish I could braze like that.
    I see that you are located in the Midwest. If you are ever in Michigan stop by and we can play with brazing.

    Quote Originally Posted by farmersammm View Post
    That is a beautiful job.
    Thanks.

    Quote Originally Posted by flushcut View Post
    "Older stuff works better most of the time and is simpler and easier to use anyway." Truer words may never have been spoken before. Old stuff rocks!
    I have stayed away from CNC and concentrated on manual machines because I wanted to learn the craft from the bottom up.

    Quote Originally Posted by Rondo View Post
    I Love repairs like this. Nice work !.
    Thanks.

    Quote Originally Posted by John T View Post
    Job selector dial makes all the difference..... Looks great.
    I agree.

    Quote Originally Posted by JJW View Post
    Don, you should give it a try with welding bi-metal blades. The toolroom where I used to work had WWWII tagged DoAll bandsaws! We would weld both high carbon & Bi-Metal blades on them. Great job on the saw!
    I might give it a try. The problem is pushing the anneal button the correct amount. Too much and the blade is soft and fails due to fatigue. Too little and the blade cools too fast and is brittle and fails immediately.

    Quote Originally Posted by bead-boy View Post
    If they were scrapping the same saw, did you try to get the table arm off it? Just in case yours gets broken again?
    The problem is timing. My friend found the selection dial about six years ago and I broke the bracket this year.

    Quote Originally Posted by Welder Dave View Post
    I'd guess the original repair wasn't heated and/or slow cooled enough because the new crack appeared right next to the braze.
    I believe that this bracket failure was due to abuse. If you look carefully the second failure occurred near but not on the edge of the first braze repair. If the saw was never abused then neither repair would be necessary.

    Quote Originally Posted by farmersammm View Post
    Maybe he shoulda G'mawed it
    If all else fails MIG it, but it would be nasty welding over the previous braze.


    Thanks,
    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  26. Likes ronsii liked this post
  27. #19
    Join Date
    Oct 2014
    Posts
    2,621
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Pic. #2 showed the crack at the edge of the braze. I agree it was from abuse or it got dropped.

  28. #20
    Join Date
    Jun 2017
    Location
    AJO, ARIZONA
    Posts
    3,364
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    The original braze job looked to me like it never fully wetted in leaving basically a cold joint. I have an old, old, old vise that my dad had, & got it from his dad, it's probably a hundred years old, anyway the moveable jaw was broken off, & grandad had brazed it back on sometime before my dad got it, it's been through HELL since we mounted it, the jaws are in reasonable alignment and its super strong. You can see how well the brazing flowed in and bonded, it's really a beautiful job.
    NRA LIFE MEMBER
    UNITWELD 175 AMP 3 IN1 DC MIG/STICK/TIG
    MIDSTATES 300 AMP AC MACHINE
    GOD BLESS AMERICA!
    “Freedom is never more than one generation away from extinction.
    We didn’t pass it to our children in the bloodstream".
    RONALD REAGAN

  29. Likes ronsii liked this post
  30. #21
    Join Date
    Mar 2008
    Location
    Georgetown, Texas
    Posts
    1,885
    Post Thanks / Like

    Re: Braze Repair on DoAll Saw

    Great repair. I have an old drill press some one gave me because the arm on the table had broken in two from being dropped. I repaired it the same way 25 years ago and still going strong.

  31. Likes ronsii liked this post

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,603,560,507.94180 seconds with 13 queries