    Wear Bar Added to Snow Blower Skid

    My friend Ray lives in the Upper Peninsula of Michigan where they get a lot of snow. He wore out the skids on his snow blower attachment to his Kubota tractor in one season. He sent me new skids and some ¼” x 3” stock. I welded the bars on the skids to extend their life. In the first picture you can see that the heel of the skid is worn almost all the way through. You will also notice that the wear wasn’t even indicating that the shoe wasn’t parallel to the ground.

    1. Worn Skid
    Name:  1. Worn Skid.jpg
Views: 341
Size:  189.5 KB

    The process that I used was:
    -I cut the ¼’ x 3” to about 10-1/2” long.
    -I scribed the corner radius on the plate and cut it out on my band saw.
    -I cleaned up the radius on my belt sander.
    -I TIG welded the wear plate to the skid in four places. I used TIG because it was all set up.
    -I clamped the skid in the vise and heated the wear bar in the area shown below with an oxyacetylene torch with a rosebud tip.

    2. Heat bending wear bar
    Name:  2. Heat bending wear bar.jpg
Views: 340
Size:  21.4 KB

    Next, I beat on the wear bar with a hammer to fit it to the skid. I decided to use the heat and beat method instead of my arbor press, because I was concerned with the bend exactly matching the existing skid. Then I MIG welded the wear bar to the skid as shown below.

    3. Wear Bar Welded
    Name:  3. Wear Bar Welded.jpg
Views: 337
Size:  153.2 KB

    Here are both skids welded.

    4. Two Skis Welded
    Name:  4. Two Skis Welded.jpg
Views: 339
Size:  152.6 KB

    Here they are primed and painted

    5. Skids primed and painted
    Name:  5. Skids primed and painted.jpg
Views: 339
Size:  106.9 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  2. Likes VaughnT liked this post
  3. #2
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    292
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Here they are installed on the snowblower.

    6. Skids installed on snowblower
    Name:  6. Skids installed on snowblower.jpg
Views: 339
Size:  67.0 KB

    On my own 1983 Simplicity tractor I am still using the skid that came with it. I just weld additional wear bars on the bottom. After about four wear bars I cut them off and start over.
    Below is a picture of my wear bar on my tractor.

    7. Simplicity skid
    Name:  7. Simplicity skid.jpg
Views: 339
Size:  99.3 KB

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  4. Likes VaughnT liked this post
  5. #3
    Join Date
    Oct 2014
    Posts
    2,606
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Really good application for some hardfacing on the bottom of the skids. Mild steel wears unbelievably fast on asphalt or concrete.

  6. Likes VaughnT liked this post
  7. #4
    Join Date
    Apr 2006
    Location
    Soda springs,Id
    Posts
    5,143
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    ^^^^^x 2^^^^
    Ol' Stonebreaker
    "Experience is the name everyone gives to their mistakes"
    Hobart G-213 portable
    Miller 175 mig
    Miller thunderbolt ac/dc stick
    Victor O/A setup
    Makita chop saw

  8. #5
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    292
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Quote Originally Posted by Welder Dave View Post
    Really good application for some hardfacing on the bottom of the skids. Mild steel wears unbelievably fast on asphalt or concrete.
    Quote Originally Posted by mla2ofus View Post
    ^^^^^x 2^^^^
    Can either of you recommend a good stick hardface rod for this application?

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250 MIG Welder
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Head Horizontal Band Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP

  9. #6
    Join Date
    Nov 2006
    Posts
    10
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Stoody 35 is a good all around rod for this. They do make wire for hardfacing as well.

  10. #7
    Join Date
    Apr 2006
    Location
    Soda springs,Id
    Posts
    5,143
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Yeah, Stoody rod lays down a nice even bead with good thickness. Just be sure to change polarity. Oh, and get out your wallet, if you know someone who works on a quarry or rock processing plant a half rack of whatever they drink will probably get you a few sticks and they will go a long way for what you're doing. It's what I use on my wheeler plow shoes.
    Ol' Stonebreaker
    "Experience is the name everyone gives to their mistakes"
    Hobart G-213 portable
    Miller 175 mig
    Miller thunderbolt ac/dc stick
    Victor O/A setup
    Makita chop saw

  11. #8
    Join Date
    Oct 2014
    Posts
    2,606
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Want something for severe abrasion but any general purpose hardfacing will work. Should be able to find in a small 1lb. pack for $25-$30. Lots of specialty rod suppliers have it in the small packages and sometimes the big box stores. It will last 4 times or more longer than mild steel. Some is run reverse polarity but hardfacing you aren't looking for maximum penetration. For those skids run beads parallel to the skids about 3/8-1/2 inch apart and you can put 2 layers for even more wear resistance. Clean the first pass with a wire brush and don't worry too much if you get a little porosity. As long as you get fusion it will work. 1/8" or 5/32" rods would be fine.
    Last edited by Welder Dave; 3 Weeks Ago at 03:29 PM.

  12. #9
    Join Date
    Mar 2005
    Location
    Under a Rock
    Posts
    5,479
    Post Thanks / Like

    Re: Wear Bar Added to Snow Blower Skid

    Nice Job Don...

    I did the same for my Dads snowblower a few years ago....

    personally, I wouldnt hard face it... 1/4" mild steel worked fine.... actually made him 2 sets... so he can swap out if necessary..... easy enough to make...
    Miller 211
    Hypertherm PM 45
    1961 Lincoln Idealarc 250
    HTP 221


    True Wisdom only comes from Pain.

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,603,275,427.00215 seconds with 15 queries