Thread: Avoiding arc start porosity on 7018?

  1. #1
    Join Date
    Oct 2013
    Location
    Long Island, NY
    Posts
    3,272
    Post Thanks / Like

    Avoiding arc start porosity on 7018?

    I never leave the nest so everything is always MIG and sometimes TIG.

    For the sake of having the ability I'm practicing on scrap here and there.

    This is 1/8" 7018 on 100 amps from a powermig 210.

    I think my beads are "decent" but the arc start is always ruined with porosity.

    I have tried starting 1/2" or so inward, and quickly whipping back once its lit as well as slowly bringing it back. Nothing I try seems to improve it.

    Name:  240802253_10158562185863231_6896021832555393193_n.jpg
Views: 1784
Size:  126.9 KB
    www.FirehouseFabricators.com

    Zach

    Millermatic 255
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  2. #2
    Join Date
    Jun 2012
    Location
    Laredo + Midland/Odessa
    Posts
    7,132
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Try 1" and slowly move it back. Make sure you get the right arc length when you get to the apart of where the bead is going to go.
    1st on WeldingWeb to have a scrolling sig!



  3. Likes BrooklynBravest, 12345678910 liked this post
  4. #3
    Join Date
    Feb 2015
    Posts
    181
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Just curious what brand of rod that is. And, a lot of times the need for clean material gets (over) stressed in my opinion, but this time it did get my attention. It looks like there is a fair amount of rust in the area where you have the porosity. Could just be how the photo looks.
    About the only suggestions I have come in the form of questions. Is the porosity coming from an unused electrode? Or from re-strikes. If it is coming from an unused electrode, the first time you use it, then it "could" be when you strike it to begin welding, your fear of sticking it to your plate is causing you to lift the electrode too high, initially giving you too much arc length.
    If porosity is coming from when you re-strike, then I would suggest grinding, filing, sanding, or whittling the end off the electrode before re-striking. Some 7018 rods seem more prone to get a mixture of molten slag and weld material glued to the end of the rod at the end of a weld, causing porosity when beginning the next pass
    But yes, the rest of your beads look fine. Don't forget that 7018 works best without any of the whipping, or forward and back motion, that is often employed with the 6010/11 electrodes.
    Good luck!

    Sent from my E6810 using http://tiny.cc/Forums_reader

  5. Likes RedOctobyr liked this post
  6. #4
    Join Date
    Feb 2019
    Location
    Snyder TX
    Posts
    642
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    My sweet spot for 1/8 7018 is 115 to 125A. Maybe a little cold @ 100A. I strike ahead of my start, long arc a little to heat the rod & stabilize the arc (engine drive), then move back to start & stuff it in to make sure I have a short arc then pause for just a micro second to let a clean puddle form. I find that a cold rod nearly always leaves a little porosity.

  7. #5
    Join Date
    Sep 2013
    Location
    central Wis.
    Posts
    6,610
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Turn your amps up. On that practice piece after a bead or 3 you would be running too hot tho. On 1/8" 7018 I would be in the 115-130 amp range depending on thickness, joint configuration and position. The 2 main causes for porosity ( excluding rust, paint or oil) are too low of amps or starting with too long of an arc.

  8. Likes BrooklynBravest liked this post
  9. #6
    Join Date
    Sep 2014
    Posts
    2,372
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by BrooklynBravest View Post
    I never leave the nest so everything is always MIG and sometimes TIG.

    For the sake of having the ability I'm practicing on scrap here and there.

    This is 1/8" 7018 on 100 amps from a powermig 210.

    I think my beads are "decent" but the arc start is always ruined with porosity.

    I have tried starting 1/2" or so inward, and quickly whipping back once its lit as well as slowly bringing it back. Nothing I try seems to improve it.

    Name:  240802253_10158562185863231_6896021832555393193_n.jpg
Views: 1784
Size:  126.9 KB
    Switch to 7016 you cannot go wrong. You can bury the rod and it just cuts deep and leaves a nice weld. It starts so nice too.

    Sincerely,

    William McCormick
    If I wasn't so.....crazy, I wouldn't try to act normal, and you would be afraid.

  10. Likes motolife313, N2 Welding liked this post
  11. #7
    Join Date
    Oct 2013
    Location
    Long Island, NY
    Posts
    3,272
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Thats a piece of HRPO 3/16" plate scrap from my plasma table.

    Its definitely not rusty or oily but I didnt take any time to prep the surface either.

    I'd prefer to learn 7018 because its such a commonly used rod. I'm literally just burning a couple rods every time I go out for practice.
    www.FirehouseFabricators.com

    Zach

    Millermatic 255
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  12. #8
    Join Date
    Oct 2015
    Location
    NW New Jersey
    Posts
    1,414
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    What are your Arc force, and Hot start settings ?

    Is your polarity correct (sometimes I have things switched around because its multi purpose, it happens occasionally), sometimes going to "Home" and going through the settings helps me remember.


    Seems a little cold amperage wise for most 1/8" 7018 work, but if you need to run that amperage( welding thinner metal and or vertical ) , increase your hot start.

    3/32" 7018 runs good 85-100 amps.

    Name:  smawoptions 210.jpg
Views: 1303
Size:  14.6 KB


    Name:  210mpchart.jpg
Views: 1311
Size:  52.5 KB

    Good luck
    Last edited by albrightree; 08-28-2021 at 10:29 AM.
    Airco 250 ac/dc Heliwelder Square wave
    Miller Synchrowave 180 sd
    Miller Econo Twin HF
    Lincoln 210 MP
    Dayton 225 ac/dc
    Victor torches
    Snap-On YA-212
    Lotos Cut60D
    Primeweld 225 ac/dc
    Primeweld mig180
    Miller AEAD-200

  13. #9
    Join Date
    Oct 2013
    Location
    Long Island, NY
    Posts
    3,272
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by albrightree View Post
    What are your Arc force, and Hot start settings ?

    Is your polarity correct (sometimes I have things switched around because its multi purpose, it happens occasionally), sometimes going to "Home" and going through the settings helps me remember.


    Seems a little cold amperage wise for most 1/8" 7018 work, but if you need to run that amperage( welding thinner metal and or vertical ) , increase your hot start.

    3/32" 7018 runs good 85-100 amps.

    Name:  smawoptions 210.jpg
Views: 1303
Size:  14.6 KB
    I messed with it a bit. I tried 115 amps, the puddle never felt like an issue it all ran smooth just the porosity.

    Hot start i tried from 3 up to 10. Arc force was 3.
    www.FirehouseFabricators.com

    Zach

    Millermatic 255
    Lincoln SW200
    Hypertherm Powermax 45xp
    2x4 CNC Plasma Table.

  14. #10
    Join Date
    Jun 2012
    Location
    CT
    Posts
    6,501
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    This is a common problem, common enough that Lincoln publishes guidance on how to avoid it

    https://www.lincolnelectric.com/en-g...ty-detail.aspx
    Miller Multimatic 255

  15. Likes BrooklynBravest, dgalo liked this post
  16. #11
    Join Date
    Dec 2013
    Posts
    2,358
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    ---Meltedmetal

  17. #12
    Join Date
    Aug 2021
    Posts
    31
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Here in Japan, we call this kind of porosity from LH rods "blow holes," and it mostly caused by what we call "start blow." Not to be confused with arc blow due to magnetic forces, but the same effect with the arc wandering around. To mitigate the effect, try starting the rod quite a bit farther forward, like maybe a full inch. After the back step, hold the rod there for a second to let the puddle build, and arc firmly establish, and keep the rod angled back. Here's a video on a A-2F qualification with LB-47 (E7016) showing the back step and rod angle. English subs, but not all clear translations...


  18. Likes BrooklynBravest, farmersammm liked this post
  19. #13
    Join Date
    Dec 2018
    Posts
    10,053
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by JDM Welder View Post
    Here in Japan, we call this kind of porosity from LH rods "blow holes," and it mostly caused by what we call "start blow." Not to be confused with arc blow due to magnetic forces, but the same effect with the arc wandering around. To mitigate the effect, try starting the rod quite a bit farther forward, like maybe a full inch. After the back step, hold the rod there for a second to let the puddle build, and arc firmly establish, and keep the rod angled back. Here's a video on a A-2F qualification with LB-47 (E7016) showing the back step and rod angle. English subs, but not all clear translations...

    That really looks nice(actually BEAUTIFUL) until the last pass. It's a bit too proud of the plate. Too much metal piled up.

    It's a booger to judge bead height in these kind of welds, been there, done that I find that viewing the puddle from the side works best, if you can get in a position to look from this angle. Flat welds can sorta suck in a way.

    Name:  clamp protection3.jpg
Views: 1458
Size:  133.8 KB See how the weld is not extremely convex, but relatively flat, but still blending nicely with the edge of the joint. A side view gives you a very good approximation of bead height.

    Name:  spike15.JPG
Views: 1253
Size:  195.3 KB

    Name:  spike18.JPG
Views: 1242
Size:  213.8 KB All welds not more than maybe 1/16 over the top of the plate.

    This is a funny!!!!!!!!!!!!!!!!!!!!!!!!!!!!!!!! Name:  spike42.JPG
Views: 1275
Size:  238.5 KB I was just starting to lose my eyesight when I made these welds. I took this pic in the mirror I think, right at the time this project was in process. I'm probably at my peak here, and that's about as good as I'll ever weld again for the remainder of my days. The welds made since, haven't been up to snuff. I'm getting closer to committing to cataract surgery I guess And I'm not keen on doing welding critique these days, because I'm not doing much better since the eyes started going.

    Anyways.............you got some good stuff there, just try to flatten out that final passName:  tkqe4fh-smiley-two-thumbs-up175028_285604.gif
Views: 1219
Size:  1.1 KB

  20. #14
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by farmersammm View Post
    That really looks nice(actually BEAUTIFUL) until the last pass. It's a bit too proud of the plate. Too much metal piled up.

    It's a booger to judge bead height in these kind of welds, been there, done that I find that viewing the puddle from the side works best, if you can get in a position to look from this angle. Flat welds can sorta suck in a way.

    Name:  clamp protection3.jpg
Views: 1458
Size:  133.8 KB See how the weld is not extremely convex, but relatively flat, but still blending nicely with the edge of the joint. A side view gives you a very good approximation of bead height.

    Name:  spike15.JPG
Views: 1253
Size:  195.3 KB

    Name:  spike18.JPG
Views: 1242
Size:  213.8 KB All welds not more than maybe 1/16 over the top of the plate.

    This is a funny!!!!!!!!!!!!!!!!!!!!!!!!!!!!!!!! Name:  spike42.JPG
Views: 1275
Size:  238.5 KB I was just starting to lose my eyesight when I made these welds. I took this pic in the mirror I think, right at the time this project was in process. I'm probably at my peak here, and that's about as good as I'll ever weld again for the remainder of my days. The welds made since, haven't been up to snuff. I'm getting closer to committing to cataract surgery I guess And I'm not keen on doing welding critique these days, because I'm not doing much better since the eyes started going.

    Anyways.............you got some good stuff there, just try to flatten out that final passName:  tkqe4fh-smiley-two-thumbs-up175028_285604.gif
Views: 1219
Size:  1.1 KB
    Go ahead and get the damned surgery. No reason to waste time. Get it. Really.

    Nice welds by the way. Thought it was MIG at first.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Last edited by 52 Ford; 08-30-2021 at 02:18 AM.
    Sent via smoke signals using my Lincoln buzzbox

  21. #15
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by BrooklynBravest View Post
    I never leave the nest so everything is always MIG and sometimes TIG.

    For the sake of having the ability I'm practicing on scrap here and there.

    This is 1/8" 7018 on 100 amps from a powermig 210.

    I think my beads are "decent" but the arc start is always ruined with porosity.

    I have tried starting 1/2" or so inward, and quickly whipping back once its lit as well as slowly bringing it back. Nothing I try seems to improve it.

    Name:  240802253_10158562185863231_6896021832555393193_n.jpg
Views: 1784
Size:  126.9 KB
    If i think about it, I'll run some 7018 tomorrow and try and make some porosity at start. I dont think I've ever had that issue.

    Damp rods, maybe? Material not clean enough? Some other contaminants on the rod? Might want to try a new pack of rods just to be sure.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Sent via smoke signals using my Lincoln buzzbox

  22. #16
    Join Date
    Jan 2004
    Location
    Brethren, Mi
    Posts
    8,959
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    They used crappy Chemtron Atom Arc on a nuke I was on, cost them millions for terrible starts.

  23. #17
    Join Date
    Dec 2015
    Posts
    132
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by farmersammm View Post
    That really looks nice(actually BEAUTIFUL) until the last pass. It's a bit too proud of the plate. Too much metal piled up.

    It's a booger to judge bead height in these kind of welds, been there, done that I find that viewing the puddle from the side works best, if you can get in a position to look from this angle. Flat welds can sorta suck in a way.

    Name:  clamp protection3.jpg
Views: 1458
Size:  133.8 KB See how the weld is not extremely convex, but relatively flat, but still blending nicely with the edge of the joint. A side view gives you a very good approximation of bead height.

    Name:  spike15.JPG
Views: 1253
Size:  195.3 KB

    Name:  spike18.JPG
Views: 1242
Size:  213.8 KB All welds not more than maybe 1/16 over the top of the plate.

    This is a funny!!!!!!!!!!!!!!!!!!!!!!!!!!!!!!!! Name:  spike42.JPG
Views: 1275
Size:  238.5 KB I was just starting to lose my eyesight when I made these welds. I took this pic in the mirror I think, right at the time this project was in process. I'm probably at my peak here, and that's about as good as I'll ever weld again for the remainder of my days. The welds made since, haven't been up to snuff. I'm getting closer to committing to cataract surgery I guess And I'm not keen on doing welding critique these days, because I'm not doing much better since the eyes started going.

    Anyways.............you got some good stuff there, just try to flatten out that final passName:  tkqe4fh-smiley-two-thumbs-up175028_285604.gif
Views: 1219
Size:  1.1 KB
    Hell just do it and be done. Cataract surgery is nothing but an office procedure these days. It’s like getting a tooth pulled . Also just like getting a tooth pulled more or less EVERYBODY is going to get it done eventually.


    Sent from my iPad using Tapatalk

  24. Likes 52 Ford, William McCormick liked this post
  25. #18
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by driz View Post
    Hell just do it and be done. Cataract surgery is nothing but an office procedure these days. It’s like getting a tooth pulled . Also just like getting a tooth pulled more or less EVERYBODY is going to get it done eventually.


    Sent from my iPad using Tapatalk
    Exactly.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Sent via smoke signals using my Lincoln buzzbox

  26. #19
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by Sberry View Post
    They used crappy Chemtron Atom Arc on a nuke I was on, cost them millions for terrible starts.
    I wonder if the ESAB Atom Arc have the same problem. I have about 40 pounds of 7018-M in sealed cans. Never burned one.

    I don't guess they would since they're still on the market.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Sent via smoke signals using my Lincoln buzzbox

  27. #20
    Join Date
    Sep 2014
    Posts
    2,372
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    If you have not tried 7016 rods they are amazing rods. You can do horizontal at 105 amp with 3/32" rods, dig in deep, and not have the puddle run. If you are doing butt joints either pipe or plate, you just leave the rod thickness gap, and it just pushes a beautiful puddle to the inside when you are overhead. You have to watch you do not push too much material if you are vertical or over the top of the weld. 7016 needs no drying out or oven, these things just go. You will not believe the penetration you get when you keep a short ARC. My friend Lou Stimberger used them and built hundreds of thousands of tons of steel docks with that rod, I heard he recently passed away but his work lives on.

    The 7016's have half the thickness of flux as the 7018's do, it is the excessive flux of the 7018 that causes that porosity.

    Sincerely,


    William McCormick
    If I wasn't so.....crazy, I wouldn't try to act normal, and you would be afraid.

  28. Likes RedOctobyr liked this post
  29. #21
    Join Date
    Oct 2014
    Posts
    5,270
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    You could try sticking the rod to the plate for a couple seconds to heat up the rod. Have done this with new rods working on pressure vessels where we took boxes of rods that weren't in the electrode oven. 7016 is not common. Some brands of 7018 are more prone to start porosity than others. I ran some 10018D2 and it was terrible for start porosity even when it came straight out of the oven.

  30. Likes 52 Ford liked this post
  31. #22
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Even if it isn't a low-hy, getting a little heat in the rod seems to always help me with stsrts.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Sent via smoke signals using my Lincoln buzzbox

  32. #23
    Join Date
    May 2012
    Location
    Ontario, Canada
    Posts
    1,505
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by BrooklynBravest View Post
    Thats a piece of HRPO 3/16" plate scrap from my plasma table.

    Its definitely not rusty or oily but I didn't take any time to prep the surface either.

    I'd prefer to learn 7018 because its such a commonly used rod. I'm literally just burning a couple rods every time I go out for practice.
    I agree with that, but I wish I'd started with a box of 7014 first.

    I was a kid, got frustrated and didn't try again for twenty years.


    I find short sessions not as helpful as a longer session.
    It takes time to get into the groove

    Wall Mountain Arc weld videos
    https://www.weldingvideos.com/







    I started by cutting rods in two or three pieces , for less twang and wobble on starts; but it also gave me more practice on arc starts too.




    Listen to the sizzle, you can really hear when you're long arcing and when it's right.

    I had huge problems with sticking the rod and
    Upping heat definitely helps

    If it's just for practice, the smaller 3/32 rod goes slower, takes less heat, gives you more rods per pound/package/dollar

    Unless you're buying the sealed tennis ball tubes, try high temp drying the rods according to the instructions, and I use a toaster oven as rod oven.
    It does make a difference.
    Last edited by 12345678910; 09-05-2021 at 11:19 AM.

  33. #24
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    Quote Originally Posted by 12345678910 View Post
    I agree with that, but I wish I'd started with a box of 7014 first.

    I was a kid, got frustrated and didn't try again for twenty years.


    I find short sessions not as helpful as a longer session.
    It takes time to get into the groove

    Wall Mountain Arc weld videos
    https://www.weldingvideos.com/







    I started by cutting rods in two or three pieces , for less twang and wobble on starts; but it also gave me more practice on arc starts too.




    Listen to the sizzle, you can really hear when you're long arcing and when it's right.

    I had huge problems with sticking the rod and
    Upping heat definitely helps

    If it's just for practice, the smaller 3/32 rod goes slower, takes less heat, gives you more rods per pound/package/dollar

    Unless you're buying the sealed tennis ball tubes, try high temp drying the rods according to the instructions, and I use a toaster oven as rod oven.
    It does make a difference.
    Impressive mustache.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Sent via smoke signals using my Lincoln buzzbox

  34. #25
    Join Date
    Dec 2020
    Location
    Virginia, USA
    Posts
    11,001
    Post Thanks / Like

    Re: Avoiding arc start porosity on 7018?

    I don't burn much 7018, so I baked about 20 pounds of them and vacuum packed them in bundles of 5 and stuck them in 10 pound cans with a little desiccant.

    I just turn the oven up to 500 and let them cook for a couple hours to dry them. Nothin' like the smell of fresh baked electrodes. Works for aluminum rods, too. I had about 250 dollars worth of those get wet and the flux turned to like a paste that wanted to peel off when I pulled the rods out the box.

    Sent from my SAMSUNG-SM-G891A using Tapatalk
    Sent via smoke signals using my Lincoln buzzbox

+ Reply to Thread

Quick Reply Quick Reply

Register Now

Please enter the name by which you would like to log-in and be known on this site.

Please enter a password for your user account. Note that passwords are case-sensitive.

Please enter a valid email address for yourself.

A) Welding/Fabrication Shop
B) Plant/Production Line
C) Infrastructure/Construction/Repair or Maintenance/Field Work
D) Distributor of Welding Supplies or Gases
E) College/School/University
F) Work Out of Home

A) Corporate Executive/Management
B) Operations Management
C) Engineering Management
D) Educator/Student
E) Retired
F) Hobbyist

Log-in

Posting Permissions

  • You may post new threads
  • You may post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,713,269,394.11187 seconds with 21 queries