    Sheet-Gauge Thickness Chart

    Thickness Weight
    Gauge Frac. Inch Dec. Inch mm oz/ft^2 lb/ft^2 kg/ft^2 kg/m^2 lb/m^2
    0000000 1/2 .5 12.7 320 20.00 9.072 97.65 215.28
    000000 15/32 .46875 11.90625 300 18.75 8.505 91.55 201.82
    00000 7/16 .4375 11.1125 280 17.50 7.983 85.44 188.37
    0000 13/32 .40625 10.31875 260 16.25 7.371 79.33 174.91
    000 3/8 .375 9.525 240 15 6.804 73.24 161.46
    00 11/32 .34375 8.73125 220 13.75 6.237 67.13 148.00
    0 5/16 .3125 7.9375 200 12.50 5.67 61.03 134.55
    1 9/32 .28125 7.14375 180 11.25 5.103 54.93 121.09
    2 17/64 .265625 6.746875 170 10.625 4.819 51.88 114.37
    3 1/4 .25 6.35 160 10 4.536 48.82 107.64
    4 15/64 .234375 5.953125 150 9.375 4.252 45.77 100.91
    5 7/32 .21875 5.55625 140 8.75 3.969 42.72 94.18
    6 13/64 .203125 5.159375 130 8.125 3.685 39.67 87.45
    7 3/16 .1875 4.7625 120 7.5 3.402 36.62 80.72
    8 11/64 .171875 4.365625 110 6.875 3.118 33.57 74.00
    9 5/32 .15625 3.96875 100 6.25 2.835 30.52 67.27
    10 9/64 .140625 3.571875 90 5.625 2.552 27.46 60.55
    11 1/8 .125 3.175 80 5 2.268 24.41 53.82
    12 7/64 .109375 2.778125 70 4.375 1.984 21.36 47.09
    13 3/32 .09375 2.38125 60 3.75 1.701 18.31 40.36
    14 5/64 .078125 1.984375 50 3.125 1.417 15.26 33.64
    15 9/128 .0703125 1.7859375 45 2.8125 1.276 13.73 30.27
    16 1/16 .0625 1.5875 40 2.5 1.134 12.21 26.91
    17 9/160 .05625 1.42875 36 2.25 1.021 10.99 24.22
    18 1/20 .05 1.27 32 2 .9072 9.765 21.53
    19 7/160 .04375 1.11125 28 1.75 .7938 8.544 18.84
    20 3/80 .0375 .9525 24 1.50 .6804 7.324 16.15
    21 11/320 .034375 .873125 22 1.375 .6237 6.713 14.80
    22 1/32 .03125 .793750 20 1.25 .567 6.103 13.46
    23 9/320 .028125 .714375 18 1.125 .5103 5.493 12.11
    24 1/40 .025 .635 16 1 .4536 4.882 10.76
    25 7/320 .021875 .555625 14 .875 .3969 4.272 9.42
    26 3/160 .01875 .47625 12 .75 .3402 3.662 8.07
    27 11/640 .0171875 .4365625 11 .6875 .3119 3.357 7.40
    28 1/64 .015625 .396875 10 .625 .2835 3.052 6.73
    29 9/640 .0140625 .3571875 9 .5625 .2551 2.746 6.05
    30 1/80 .0125 .3175 8 .5 .2268 2.441 5.38
    31 7/640 .0109375 .2778125 7 .4375 .1984 2.136 4.71
    32 13/1280 .01015625 .25796875 6 1/2 .40625 .1843 1.983 4.37
    33 3/320 .009375 .238125 6 .375 .1701 1.831 4.04
    34 11/1280 .00859375 .21828125 5 1/2 .34375 .1559 1.678 3.70
    35 5/640 .0078125 .1984375 5 .3125 .1417 1.526 3.36
    36 9/1280 .00703125 .17859375 4 1/2 .28125 .1276 1.373 3.03
    37 17/2560 .006640625 .168671875 4 1/4 .265625 .1205 1.297 2.87
    38 1/160 .00625 .15875 4 .25 .1134 1.221 2.69
    Last edited by vipermanz; 07-25-2005 at 05:15 PM.


    Stangnet
    Shop Full Of Stuff.

    Joey

  2. #2
    Join Date
    Oct 2003
    Location
    Birmingham Al
    Posts
    750
    Post Thanks / Like

  3. #3
    Join Date
    Jul 2005
    Location
    ohio
    Posts
    43
    Post Thanks / Like

    ???

    Just out of curiosity does anyone know what gauge aluminum foil is?

  4. #4
    Join Date
    Feb 2005
    Location
    Las Vegas
    Posts
    9
    Post Thanks / Like
    atrain,
    According to the Aluminum Association;
    aluminum foil is considered "less than .006"
    plate = 1/4" or more
    sheet = .249" to .006"
    foil = less than .006"
    I just found this out last night, then I see this post today, so there you have it .

  5. #5
    Join Date
    Jul 2005
    Location
    ohio
    Posts
    43
    Post Thanks / Like
    thanks chuck

  6. #6
    Join Date
    Apr 2006
    Location
    Florida
    Posts
    41
    Post Thanks / Like

    Printable table in Word

    Great information, thanks. I formatted it into Word so I could print and post it. Sheez, allergies, keep me up all night....

    Okay, I made the file smaller, so I could upload it. You can put your own title on it.
    Attached Files Attached Files
    Last edited by Bobcatter; 04-16-2006 at 02:10 AM.

  7. #7
    Join Date
    Jul 2006
    Location
    Washington State in the San Juan Islands
    Posts
    8
    Post Thanks / Like

    Re: Printable table in Word

    Thanks - for your efforts getting all the info to line up in "word". A real good refernce!

  8. #8
    Join Date
    Jun 2005
    Location
    Taberg, NY ( near Syracuse )
    Posts
    137
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Does anyone know what the gauge of typical car body metal is ?
    Uhmmm particuliarly the older vehicles like a TR-8 ??

  9. #9
    Join Date
    Aug 2006
    Location
    near rochester NY
    Posts
    1,195
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    newer cars can go to 26gage but most older are closer to 18.
    thanks for the chart, verry helpfull.

    summer is here, plant a tree for mother earth. if you dont have time or space, sponcer some one else to plant one for you.

    feel free to shoot me a PM or e-mail me at [email]james@newyorkmetalart.com i got lots of time.

  10. #10
    Join Date
    Jan 2005
    Location
    Indiana
    Posts
    59
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Had to save that. Thanks for the chart!

  11. #11
    Join Date
    Apr 2006
    Location
    Soda springs,Id
    Posts
    5,735
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    My thanks to Vipermanz and Bobcatter for the chart. I printed off 2,one for my shop and one to make bets on how thick 10 ga is. Everyone i've ever talked about it w/ has always said it is 1/8", including myself!!!!
    Thanks again,
    Mike
    Ol' Stonebreaker
    "Experience is the name everyone gives to their mistakes"
    Hobart G-213 portable
    Miller 175 mig
    Miller thunderbolt ac/dc stick
    Victor O/A setup
    Makita chop saw

  12. #12
    Join Date
    Oct 2006
    Posts
    48
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    i allways thought 10 gauge was 3.2mm thats what the old guys refer to in old money welding rods 12 gauge was 2.5

  13. #13
    Join Date
    Aug 2006
    Location
    Middleburg, FL USA
    Posts
    72
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    I found this online at davesport.com

    Grade and Description Chemistry Tensile Yield Rockwell Hardness
    Units typical ksi ksi typical
    1010
    ERW tube C .08-.13
    Mn .30-.60
    P .035 max
    S .035 max
    45 32 RB55 min
    1020
    DOM tube C .15-.25
    Mn .30-.60
    P .040 max
    S .050 max
    80 70 RB80
    4130
    DOM tube
    (chromoly) C .28-.33
    Mn .40-.60
    P .035
    S .040
    Si .15-.35
    Cr .80-1.10
    Mo .15-.25
    100 90 RB90

    As you can see, DOM tubing is nearly twice as strong in tension, and more than twice as strong in resistance to bending in comparison to the ERW tube. Also, the 4130 chromoly tube is only 20% stronger than standard DOM in tension.

    Weights of typical tubing sizes

    Outside Diameter Wall thickness Inside Diameter Type Weight, lbs/ft. Wgt/80ft.
    1.25" 0.120 1.010" HREW/DOM 1.448 116
    1.375" 0.120 1.135" HREW/DOM 1.608 128.6
    1.5" 0.095" 1.310 HREW/DOM 1.426 114
    1.5" 0.120" 1.260" HREW/DOM 1.769 141.5
    1.75" 0.109" (FIA) 1.532" DOM 1.910 152.8
    1.75" 0.120" 1.510" HREW/DOM 2.089 167.1



    Gauge
    Number
    Thickness (Inches)
    Pounds Per Sq. Ft.

    Nominal
    Tolerance Range

    10
    .1345
    .1405 to .1285
    5.48695

    11
    .1196
    .1256 to .1136
    4.87911

    12
    .1046
    .1106 to .0986
    4.26718

    13
    .0897
    .0947 to .0847
    3.65933

    14
    .0747
    .0797 to .0697
    3.04740

    15
    .0673
    .0723 to .0623
    2.74552

    16
    .0598
    .0648 to .0548
    2.43955

    17
    .0538
    .0578 to .0498
    2.19478

    18
    .0478
    .0518 to .0438
    1.95001

    19
    .0418
    .0458 to .0378
    1.70524

    20
    .0359
    .0389 to .0329
    1.46455

    21
    .0329
    .0359 to .0299
    1.34216

    22
    .0299
    .0329 to .0269
    1.21978

    23
    .0269
    .0299 to .0239
    1.09739

    24
    .0239
    .0269 to .0209
    .97501

    25
    .0209
    .0239 to .0179
    .85262

    26
    .0179
    .0199 to .0159
    .73023

    27
    .0164
    .0184 to .0144
    .66094
    Always looking for another old VW, especially in the southeast.

  14. #14
    Join Date
    Dec 2004
    Location
    Saudi Arabia
    Posts
    3
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Thanks guys
    Great infos

  15. #15
    Join Date
    Aug 2007
    Posts
    46
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Can someone PLEASE explain to me why I didn't find this message board until last week, when I really needed all this info 3 weeks ago???



    Hee Hee

  16. #16
    Join Date
    Oct 2007
    Posts
    247
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Great info...

    Saving most of it...

  17. #17
    Join Date
    Aug 2006
    Location
    near rochester NY
    Posts
    1,195
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    well at first glance one would think this is very helpful. BUT all it really dose if confuse you even more ???
    none of the #'s match ???what chart do we trust ??

    vipermanz...............VS................bugdust

    COLOR="blue"]vipermanz[/COLOR]...............
    20 3/80 .0375
    27 11/640 .0171875
    15 9/128 .0703125

    VS................bugdust

    20 .0359
    27 .0164
    15 .0673


    at first i just thought it was a simple question of rounding it up to keep the # from going on forever, but???? 20 gage .0375 and 20 gage .0359 are way to far to be rounding for simplicity sake ?? so what gives ?? must be a tolerance thing ??
    the only solution i see is ....

    summer is here, plant a tree for mother earth. if you dont have time or space, sponcer some one else to plant one for you.

    feel free to shoot me a PM or e-mail me at [email]james@newyorkmetalart.com i got lots of time.

  18. #18
    Join Date
    Jan 2008
    Location
    Arkansas
    Posts
    1,202
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Name:  chart.jpg
Views: 21759
Size:  117.4 KB
    blow this up 2x to read it
    Last edited by Magnetic Mechanic; 01-31-2008 at 12:29 PM. Reason: no explanation

  19. #19
    Join Date
    Jan 2008
    Location
    Port Jervis, NY
    Posts
    196
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    very helpful!!!!! printed a copy for the tool box... Thanks everyone

  20. #20
    Join Date
    Aug 2008
    Posts
    1
    Post Thanks / Like

    Smile I was to hasty in my previous reply.

    In the start window I get the button 'Try It' which I clicked. But it still ends after 10 minutes.

  21. #21
    Join Date
    Dec 2007
    Location
    Reno, NV
    Posts
    61
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Just to point out ferrous metal sheet and aluminum sheet gauge numbers refer to different thicknesses, meaning 10 ga. steel sheet is different thickness that 10 ga aluminum sheet. Though there are several good sources on the web, I like Aircraft Spruce and Specialty's info sheets out of their online catalog. The catalog is worth having just for the info, just like the old Starrett catalogs, verituble encyclopedias of measuring and setup info. Try this page:
    http://www.aircraftspruce.com/catalo...metalinfo1.php

  22. #22
    Join Date
    Apr 2008
    Location
    Charlotte NC
    Posts
    919
    Post Thanks / Like

    Re: Printable table in Word

    Quote Originally Posted by Bobcatter View Post
    Great information, thanks. I formatted it into Word so I could print and post it. Sheez, allergies, keep me up all night....

    Okay, I made the file smaller, so I could upload it. You can put your own title on it.
    thinks guy for the printable info. I had written down the common guages used and posted it on my tool box for purchasing info. This is more better. Thanks again.
    Miller TrailBlazer 251
    Miller HF-250-1
    Miller MaxStar 150 STL
    HyperTherm PowerMax 380 plasma
    Lincoln PowerMig 180
    Millermatic 252
    Miller Diversion 180

  23. #23
    Join Date
    Jun 2008
    Location
    Central California
    Posts
    5,801
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Machinery's Handbook has these plus other 'odd' and British standards too. It is a very good reference book, although having the chart printed out for your wall or toolbox is also a great idea.
    Well, after doing a search here, I see that the Handbook has been mentioned on site fairly regularly, so I won't say more now.

  24. #24
    Join Date
    Apr 2008
    Location
    Delaware
    Posts
    86
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    The chart is going on my wall and I will be handing out copies to my students....It well be a lesson in the making...I always used my pipe fitting book to look up thicknesses...this chart puts all the info in one spot...THANKS
    Jonesy

  25. #25
    Join Date
    Nov 2007
    Location
    Pittsburgh Pennsylvania
    Posts
    1,330
    Post Thanks / Like

    Re: Sheet-Gauge Thickness Chart

    Wow all this time and i didnt even notice this thread. I just printed one out. Thanks alot!!!
    Ya gotta spend money to make money!

+ Reply to Thread

Quick Reply Quick Reply

Register Now

Please enter the name by which you would like to log-in and be known on this site.

Please enter a password for your user account. Note that passwords are case-sensitive.

Please enter a valid email address for yourself.

A) Welding/Fabrication Shop
B) Plant/Production Line
C) Infrastructure/Construction/Repair or Maintenance/Field Work
D) Distributor of Welding Supplies or Gases
E) College/School/University
F) Work Out of Home

A) Corporate Executive/Management
B) Operations Management
C) Engineering Management
D) Educator/Student
E) Retired
F) Hobbyist

Log-in

Posting Permissions

  • You may post new threads
  • You may post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,713,294,977.88531 seconds with 19 queries