    I just started a new job, and the first task is a kinda interesting one, a 6 way blade off of a D5 dozer that has been beat to **** and needs some love.

    I didn't get any pics of the start of the job, but a heap of crack repairs, and the primary spherical bearing boss had been completely *ahem* "removed" somehow.

    So crack repairs and a new bearing boss.

    The overview, had a heap of crack repairs to do around the mounts for the blade angle lugs, the doubler skin and the stick rake attachment lugs on the bottom.



    The stick rake attachments were an in the field modification, and whoever welded them on didnt like overhead so they only did one tiny (like 1/8th) fillet weld on all the overheads, so of course they all cracked, with all of the dirt, paint, rust and crud built up MIG wasnt going to be an option, I ground a groove and run a small hot root pass with a 1/8 6010 to try and burn out as much of the crap, then a 3 run fillet with 7016 over the 6010 on the gusset plates.



    And some overhead, not as neat, but its been 6 months since I've run stick, and 12 since I've run 7016.



    and some vertical up as well, same deal 6010 root, 7016 over the top.



    The factory weld's on this doubler plate has some nasty undercut on the top toe of the weld which caused it to crack, I oxy/LPG gouged that out and re welded it with the MIG, no idea what settings as it's a 30 year old WIA machine with no read outs, but felt like around 35 volts and 650 IPM of wire.



    Same thing here, undercut on the weld toe leading to cracking but the repair is welded vertical up with the MIG this time.



    These weld's failed for a different reason, massive porosity, like full on aero bar bubbly **** when I gouged it out.



    And the reason the blade came in at all, somehow they managed to rip out the 2 inch thick main bearing boss, so machined with the line boring bar ready to have a new boss welded in.


  2. #2
    Join Date
    Dec 2018
    Posts
    4,726
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    Geez, THAT'S NICE. I can't do that quality of work.

  3. Likes driz liked this post
  4. #3
    Join Date
    Apr 2016
    Posts
    364
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    What a great description, don't even need a photo! A carbonated chocolate bar, why.. ,, ..... Do they still make Aero Bars???

  5. #4
    Join Date
    Mar 2012
    Location
    Australia
    Posts
    653
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    Quote Originally Posted by Weldalittle View Post
    What a great description, don't even need a photo! A carbonated chocolate bar, why.. ,, ..... Do they still make Aero Bars???
    Yeah, maybe its not the same aero bars as in other countries, but they're still pretty popular here.

    https://www.woolworths.com.au/shop/p...milk-chocolate

  6. #5
    Join Date
    Sep 2007
    Location
    Gold Coast, Australia
    Posts
    237
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    great work!.... but now I want an aero bar

  7. #6
    Join Date
    Apr 2016
    Posts
    364
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    Quote Originally Posted by ttoks View Post
    Yeah, maybe its not the same aero bars as in other countries, but they're still pretty popular here.

    https://www.woolworths.com.au/shop/p...milk-chocolate
    Different than what I am familiar with, but same porosity...

    https://encrypted-tbn0.gstatic.com/i...4eWZA&usqp=CAU

  8. #7
    Join Date
    May 2017
    Location
    Pitman PA
    Posts
    728
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    Thats some nice lookin work you do there ttok, its always fun too take a beat up ol diggin device and make it useful again, we get our share of it here in the anthracite regions and I enjoy the challenge. Ive always said you got the money I got the time

  9. #8
    Join Date
    Dec 2010
    Location
    SoCal-LA
    Posts
    9,793
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    I love your work, your photos, your commentary.

    Nice work!
    Weld like a "WELDOR", not a wel-"DERR"
    MillerDynasty700DX,Dynasty350DX4ea,Dynasty200DX,Li ncolnSW200-2ea.,MillerMatic350P,MillerMatic200w/spoolgun,MKCobraMig260,Lincoln SP-170T,PlasmaCam/Hypertherm1250,HFProTig2ea,MigMax1ea.

  10. #9
    Join Date
    Jun 2012
    Location
    Sebeka and Bemidji MN
    Posts
    14,765
    Post Thanks / Like

    Re: CAT D5 6 way blade repair

    Threads like this are great - they remind me why I like to weld

    ...all I get is mostly boring stuff...
    Dave J.

    Beware of false knowledge; it is more dangerous than ignorance. ~George Bernard Shaw~

    Syncro 350
    Invertec v250-s
    Thermal Arc 161 and 300
    MM210
    Dialarc
    Tried being normal once, didn't take....I think it was a Tuesday.

  11. #10
    Join Date
    Jan 2017
    Location
    Dallas, TX
    Posts
    57
    Post Thanks / Like

    CAT D5 6 way blade repair

    Excellent write up! When you said aero bar, this is what came to mind for me LOL.


    Sent from my iPhone using Tapatalk

Posting Permissions

  • You may not post new threads
  • You may not post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,620,900,808.11668 seconds with 14 queries