    Welding of Boat Hoist Brackets

    My friend and customer Mark owns a home on Lake Saint Claire here in Michigan. Recently the water level of the lake has been very high. The problem is that his boat hoist can’t lift the carriage that holds the boat high enough to get the carriage out of the waves. This causes the waves to beat the carriage to death. The boat hoist is constructed of four pylons. The two pylons on the right have winches on them and the two on the left have idler pullies on them. The winch has enough travel to lift the carriage of the boat hoist out of the waves but the idler side can’t keep up, because the cable will rub on the flame cut hole in the channel iron of the dock. The hole is already fairly large so it is undesirable to make it any larger, without compromising the integrity of the dock. Mark’s solution was to design a different bracket to hold the idler, which put the cable out far enough to entirely clear the channel iron. The first picture shows the entire dock.

    1. Boat dock-1
    Name:  1. Boat dock-1.jpg
Views: 680
Size:  116.7 KB

    The next picture is a close up which shows the winches on the right and the idler pullies on the left.

    2 Boat dock-2
    Name:  2 Boat dock-2.jpg
Views: 689
Size:  83.9 KB

    The third picture shows a close up of the original idler bracket. You can see that part of the problem is that the cable from the pulley to the cross brace of the carriage isn’t vertical. As the carriage is raised the angle of the cable causes it to get closer and eventually rub on the flame cut hole in the channel iron.

    3. Boat dock-3
    Name:  3. Boat dock-3.jpg
Views: 707
Size:  20.5 KB

    My task is to weld on the new brackets on the idler side of the boat hoist as shown below. Unfortunately, the dock on the idler side is only 18 inches wide.

    4. Hoist site view
    Name:  4. Hoist site view.jpg
Views: 680
Size:  60.1 KB

    The next three pictures show the bracket that needs to be welded to the pylon. The required weld is shown in purple. The cable is shown in red and as you can see it is well away from the channel and vertical.

    5. Bottom view of bracket
    Name:  5. Bottom view of bracket.jpg
Views: 685
Size:  47.8 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  2. #2
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    6. weld view1
    Name:  6. weld view1.jpg
Views: 668
Size:  37.2 KB

    7. weld view 2
    Name:  7. weld view 2.jpg
Views: 668
Size:  31.3 KB

    The pylons were driven 30 years ago and the pipes weren’t new when they were driven. The pylon closest to the shore was in very good shape.

    8. Land side pylon
    Name:  8. Land side pylon.jpg
Views: 669
Size:  54.8 KB

    The next two pictures show that the offshore pylon was a little pitted from rust.

    9. Offshore pylon 1
    Name:  9. Offshore pylon 1.jpg
Views: 651
Size:  51.3 KB

    10. Offshore pylon 2
    Name:  10. Offshore pylon 2.jpg
Views: 662
Size:  61.3 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  3. #3
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    This is a picture of me welding the offshore bracket to the pylon.

    11. Welding bracket
    Name:  11. Welding bracket.jpg
Views: 667
Size:  135.5 KB

    Before I welded the bracket, I tack welded the four corners to keep it from moving during welding.

    12.Tack-1
    Name:  12.Tack-1.jpg
Views: 660
Size:  65.8 KB

    13. Tack-2
    Name:  13. Tack-2.jpg
Views: 661
Size:  77.2 KB

    14. Tack 3
    Name:  14. Tack 3.jpg
Views: 675
Size:  70.1 KB

    The first pass was done with the following:

    Vertical plate: ½” thick
    Tube: Ø8-1/2 5/16” thick

    Rod: 3/32” 6011
    Current: 80 amps
    Polarity: DCEP
    Dig: 50%
    Motion: Whip and pause with slight wiggle on the bottom forming an inverted Tee.

    15. First pass
    Name:  15. First pass.jpg
Views: 664
Size:  83.0 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  4. Likes farmersammm liked this post
  5. #4
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    The second pass was done with the following:

    Rod: 1/8” 7018
    Current: 105 amps
    Polarity: DCEP
    Dig: 30%
    Motion: Inverted Vee

    16. Second pass
    Name:  16. Second pass.jpg
Views: 664
Size:  81.5 KB

    I beveled the ¼” top plate at a 30° angle. It had a 3/32” root gap.

    The first pass was done with the following.

    Rod: 3/32” 6011
    Current: 80 amps
    Polarity: DCEP
    Dig: 50%
    Motion: Whip and pause

    The second pass was done with the following:

    Rod: 5/32” 7018
    Current: 140 amps
    Polarity: DCEP
    Dig: 30%
    Motion: Cursive U’s

    17. Top Weld
    Name:  17. Top Weld.jpg
Views: 665
Size:  110.8 KB

    The left side weld parameters were similar to the right-side weld.

    18. left side pylon-1
    Name:  18. left side pylon-1.jpg
Views: 663
Size:  82.4 KB

    19. Left side pylon-2
    Name:  19. Left side pylon-2.jpg
Views: 650
Size:  73.8 KB

    I also patched the original hole in the channel iron.

    20. Patch
    Name:  20. Patch.jpg
Views: 682
Size:  113.8 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  6. Likes farmersammm liked this post
  7. #5
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Here is a picture of the offshore pylon with the new bracket welded in place.

    21. Offshore pylon done
    Name:  21. Offshore pylon done.jpg
Views: 657
Size:  85.6 KB

    Here is a picture of the Land side pylon with the new bracket welded in place.

    22. Land side pylon done
    Name:  22. Land side pylon done.jpg
Views: 666
Size:  86.0 KB

    Here is a close up of the two pylons with the new idler brackets welded in place.

    23. two pylons done
    Name:  23. two pylons done.jpg
Views: 678
Size:  88.3 KB

    Here is the boat hoist all done.

    24. Boat hoist done
    Name:  24. Boat hoist done.jpg
Views: 749
Size:  96.5 KB

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  8. Likes frieed, Beefman, Shootr, farmersammm, whtbaron liked this post
  9. #6
    Join Date
    Sep 2005
    Location
    Cave Creek AZ
    Posts
    3,347
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Looks a little cold, what did you end up using for a welder and power source.

  10. #7
    Join Date
    Oct 2019
    Location
    Australia
    Posts
    783
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Good job and nicely documented. Thanks for sharing.

  11. #8
    Join Date
    Oct 2014
    Posts
    5,270
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    I agree with a little cold on the 7018. Normally for vertical up with 1/8" you'd be 120+ amps. 5/32" would be 150+ amps.

  12. #9
    Join Date
    Oct 2015
    Location
    NW New Jersey
    Posts
    1,414
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Great Job ! The project looks like it came out well. The welds came out nice, how long did you have to practice ? Did you find someone to give you pointers, or did you figure it out on your own? You mention Dig Control percentage, so I guess you didn't use the 210MP it uses arc force 1-10. Did you use the Dynasty, or maybe an engine drive ?
    I hope you get some time on the lake as well getting paid. It looks beautiful out there.

    Best Regards
    Airco 250 ac/dc Heliwelder Square wave
    Miller Synchrowave 180 sd
    Miller Econo Twin HF
    Lincoln 210 MP
    Dayton 225 ac/dc
    Victor torches
    Snap-On YA-212
    Lotos Cut60D
    Primeweld 225 ac/dc
    Primeweld mig180
    Miller AEAD-200

  13. #10
    Join Date
    Feb 2019
    Location
    Snyder TX
    Posts
    643
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Got 'er done!

  14. #11
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Quote Originally Posted by walker View Post
    Looks a little cold, what did you end up using for a welder and power source.
    For power, we used the 240 volt 30 amp circuit out on the dock that was provided for the two hoists.
    For a welder I used my Miller Dynasty 200 DX. In the following picture you can see the equipment and Mark grinding the paint off the area around the patch.

    25. Mark and equipment on dock
    Name:  25.  Mark and equipment on dock.jpg
Views: 756
Size:  130.9 KB

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  15. Likes whtbaron liked this post
  16. #12
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Quote Originally Posted by Welder Dave View Post
    I agree with a little cold on the 7018. Normally for vertical up with 1/8" you'd be 120+ amps. 5/32" would be 150+ amps.
    Dave, Thanks for taking time to comment. I know that you are facing some health challenges. I will try some samples with the hotter settings as you recommend.

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  17. #13
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Quote Originally Posted by Woznme View Post
    Good job and nicely documented. Thanks for sharing.
    Thanks,
    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  18. #14
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Quote Originally Posted by albrightree View Post
    Great Job ! The project looks like it came out well. The welds came out nice, how long did you have to practice ?
    I practiced about 60 hours over a period of 8 month, while waiting for a sunny day with light wind. Here is a picture of my practice pieces.
    Name:  IMG_9188.jpg
Views: 509
Size:  144.2 KB

    Did you find someone to give you pointers, or did you figure it out on your own? You mention Dig Control percentage, so I guess you didn't use the 210MP it uses arc force 1-10.
    I wound up using the Dynasty 200 DX.

    Did you use the Dynasty, or maybe an engine drive ?
    I connected the Dynasty to the 30 amp 240 volt circuit that was out on the dock to power the two winches.

    I hope you get some time on the lake as well getting paid. It looks beautiful out there.
    Mark invited me to share lunch and dinner with his family on the covered deck that was on the back of his house. It was very peaceful.

    Name:  IMG_9114.jpg
Views: 520
Size:  102.4 KB

    Name:  IMG_9115.jpg
Views: 513
Size:  114.3 KB
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  19. Likes Shootr, farmersammm liked this post
  20. #15
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Mark primed the welded area and hooked up the cables. It worked as expected. Here are a few pictures.

    Name:  IMG_0757.jpg
Views: 538
Size:  91.7 KB

    Name:  IMG_0758.jpg
Views: 516
Size:  63.1 KB

    Name:  IMG_0759.jpg
Views: 524
Size:  61.8 KB

    Mark said that he was going to remove the pulleys that provide side tension to the cables, which are shown below, because they no longer serve any purpose.
    Name:  IMG_0760.jpg
Views: 509
Size:  99.5 KB

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  21. Likes farmersammm, whtbaron liked this post
  22. #16
    Join Date
    Mar 2014
    Location
    Troy MI
    Posts
    922
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Mark also said that the hoist now lifts the boat high enough to get the carriage that holds the boat out of the waves. Yipee.

    -Don
    Smith Oxyacetylene Torch
    Miller Dynasty 200DX
    Lincoln SP-250
    Clausing/Coldchester 15" Lathe
    16" DuAll Saw
    15" Drill Press
    7" x 9" Swivel Mast Saw
    20 Ton Arbor Press
    Bridgeport
    Lincoln LE 31 MP & Lincoln 210 MP
    Everlast PowerTIG 400 EXT

  23. Likes Shootr liked this post
  24. #17
    Join Date
    May 2007
    Posts
    4,589
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    u must trust urself, more than i do myself, not to kick that expensive inverter into the water. i got some of that flat braided rope commercial electicians use to pull wire permenrtly looped through the handle on mine, and that baby gets tied to columns, sizzor lifts, rails, pipe racks on truck, etc, cuz i dont trust myself or others around. actually i woulda ran leads out there, and tied it to dry land. it looks really good, i mean real good, considering it wasnt so long ago, u said u werent usedto stick welding. i probably brought brackes down an inch or so lower for sake of pipes ends, and woulda hit weld area w/ hard grinding wheel before, as some of pipe his seen the environment. also, that jacket u got to protect your knees/legs, is nicer than the one i get to wear
    Last edited by 123weld; 07-27-2021 at 07:18 PM.

  25. Likes walker liked this post
  26. #18
    Join Date
    Feb 2016
    Location
    Myrtle Beach
    Posts
    899
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Always enjoy your threads. Nicely Done!
    Lincoln 350MP
    Millermatic 350P
    Syncrowave 250
    1969 SA200
    HTP Invertig 221

  27. #19
    Join Date
    Mar 2018
    Location
    Sechelt, BC
    Posts
    475
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Get rid of that crappy steel cable and get some Amsteel or Dyneema.
    Do not believe everything that you think.

  28. #20
    Join Date
    Mar 2018
    Location
    Sechelt, BC
    Posts
    475
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Sorry, very rude of me, I meant to say how good your project looked. Nicely done!
    Do not believe everything that you think.

  29. #21
    Join Date
    Jan 2011
    Location
    W. Wisc
    Posts
    939
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Quote Originally Posted by 123weld View Post
    u must trust urself, more than i do myself, not to kick that expensive inverter into the water. i got some of that flat braided rope commercial electicians use to pull wire permenrtly looped through the handle on mine, and that baby gets tied to columns, sizzor lifts, rails, pipe racks on truck, etc, cuz i dont trust myself or others around.
    LOL - I was going to say the same thing. That picture with the welder behind your friend's feet made me cringe for that reason. Very nice work, as always!
    -Dave
    XMT304 with: 22A Feeder, or HF251 Hi Freq DC TIG air cooled

  30. Likes whtbaron liked this post
  31. #22
    Join Date
    Dec 2018
    Posts
    10,053
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    Screw the welder!! I'd be tying myself to the dock Homeboy doesn't know how to swim.

  32. Likes whtbaron, Lis2323 liked this post
  33. #23
    Join Date
    May 2014
    Location
    Manitoba Canada
    Posts
    14,977
    Post Thanks / Like

    Re: Welding of Boat Hoist Brackets

    LOL.... must be a dryland farmer thing. I'm a natural boat anchor as well...
    250 amp Miller DialArc AC/DC Stick
    F-225 amp Forney AC Stick
    230 amp Sears AC Stick
    Lincoln 180C MIG
    Vevor MIG 200A
    Victor Medalist 350 O/A
    Vevor Cut 50 Plasma
    Les

  34. Likes farmersammm, Lis2323 liked this post
+ Reply to Thread

Quick Reply Quick Reply

Register Now

Please enter the name by which you would like to log-in and be known on this site.

Please enter a password for your user account. Note that passwords are case-sensitive.

Please enter a valid email address for yourself.

A) Welding/Fabrication Shop
B) Plant/Production Line
C) Infrastructure/Construction/Repair or Maintenance/Field Work
D) Distributor of Welding Supplies or Gases
E) College/School/University
F) Work Out of Home

A) Corporate Executive/Management
B) Operations Management
C) Engineering Management
D) Educator/Student
E) Retired
F) Hobbyist

Log-in

Posting Permissions

  • You may post new threads
  • You may post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,713,285,866.16076 seconds with 22 queries