    Welding with 6010+ on either straight or reverse polarity is pretty difficult on my machine. The arc likes to extinguish frequently, and to maintain the arc as best as possible, I'm finding that I have to bury the tip of the rod in the molten flux puddle.
    6011 will run completely fine at the same amperage (on AC).
    Is this some inherent fault of my machine, or do I need to adjust something?
    IWW member
    Century: 250 amp AC/DC, 295 amp AC, High Frequency Box
    Victor, Harris, and Oxweld Oxy-Acetylene Equipment.

  2. #2
    Join Date
    Jun 2012
    Location
    CT
    Posts
    6,501
    Post Thanks / Like

    Re: Issue with 6010 arc

    Some machines, especially small inverters, don't run 6010 very well. Just not enough voltage on the output. Stick to 6011 or try a different welder if you really have to use 6010

  3. #3
    Join Date
    Apr 2021
    Location
    Adelaide, South Australia
    Posts
    431
    Post Thanks / Like

    Re: Issue with 6010 arc

    If you have VRD can you disable it? It might help.

    Try not to electrocute yourself though.

    Jack

  4. #4
    Join Date
    Oct 2015
    Location
    NW New Jersey
    Posts
    1,414
    Post Thanks / Like

    Re: Issue with 6010 arc

    What machine are you running it on ? What are your settings ? Are you using Lincoln 6010+ ( the grey stuff) not the Red electrodes. What is your Primary ( input ) voltage 230v,240v, maybe 208v ?

    I have a Dayton 250 AC/DC that is probably very similar to you Century, and running 230 vac it runs 6010 but is very sticky/cranky. On 208 vac without changing internal taps its near impossible to run, moving taps helps but its a bit of a job to keep a steady arc.
    When running 6010 on my EconoTwinHF or Airco250 both run good on 230v, but I can tell when I'm running on 208v(without changing taps) its a little bit cranky, and I have to turn up the amps just a little bit to compensate. All the other rods run fine 6011, 6013,7014,7018, 308,309,316,NI55, and some maintanence rods.


    My point is , input voltage can affect how your machine will run 6010, almost as much as what machine you run it on. Some machines (even transformer) just don't run 6010 as well as others. If you have a job that spec's that rod, you might need to get a machine that works well with 6010. None of my work has 6010 specified , but I do have some of the red, and some of the grey in the shop.



    I solved the problem by buying a 50lb box of Lincoln 1/8" 6011, and it works everywhere, with every thing.


    Good luck
    Last edited by albrightree; 10-07-2021 at 09:13 AM.
    Airco 250 ac/dc Heliwelder Square wave
    Miller Synchrowave 180 sd
    Miller Econo Twin HF
    Lincoln 210 MP
    Dayton 225 ac/dc
    Victor torches
    Snap-On YA-212
    Lotos Cut60D
    Primeweld 225 ac/dc
    Primeweld mig180
    Miller AEAD-200

  5. #5
    Join Date
    Apr 2006
    Location
    Soda springs,Id
    Posts
    5,735
    Post Thanks / Like

    Re: Issue with 6010 arc

    I have some 6010 that was given to me and I have to turn up the amps a little on my Miller Thunderbolt to run 6010. I think the OCV is a little too low for this.
    Ol' Stonebreaker
    "Experience is the name everyone gives to their mistakes"
    Hobart G-213 portable
    Miller 175 mig
    Miller thunderbolt ac/dc stick
    Victor O/A setup
    Makita chop saw

  6. #6
    Join Date
    Mar 2018
    Location
    Clovis California
    Posts
    9,896
    Post Thanks / Like

    Re: Issue with 6010 arc

    You all welding rod type and has different technic. It will even change with welding machines.

    If you can weld with E6011 why not use E6011. They both high pen rod the only difference is E6010 is DC only and E6011 is both AC and DC

    Dave

    Quote Originally Posted by Carbon-Arc View Post
    Welding with 6010+ on either straight or reverse polarity is pretty difficult on my machine. The arc likes to extinguish frequently, and to maintain the arc as best as possible, I'm finding that I have to bury the tip of the rod in the molten flux puddle.
    6011 will run completely fine at the same amperage (on AC).
    Is this some inherent fault of my machine, or do I need to adjust something?

  7. Likes lugweld, John Baptist, CAVEMANN liked this post
  8. #7
    Join Date
    Jun 2021
    Posts
    132
    Post Thanks / Like

    Re: Issue with 6010 arc

    To answer all questions:
    I'm running the 6010 on the Century 250 amp AC/DC transformer machine.
    The 6010 is the Lincoln grey rod.
    No VRD on my machine.
    I'm not sure about input voltage, my plugin is one of those four prong explodable types.
    I had initially dismissed too low OCV, since I can maintain some pretty long arc lengths with other rods, but maybe I'm mistaken.
    I'll be back to welding on Friday, I'll play around with the 6010 a little more. I did find that welding with it was much easier of I stick the rod and let it heat up for 10 seconds before striking the arc.
    IWW member
    Century: 250 amp AC/DC, 295 amp AC, High Frequency Box
    Victor, Harris, and Oxweld Oxy-Acetylene Equipment.

  9. #8
    Join Date
    Oct 2015
    Location
    NW New Jersey
    Posts
    1,414
    Post Thanks / Like

    Re: Issue with 6010 arc

    Quote Originally Posted by Carbon-Arc View Post
    To answer all questions:
    I'm running the 6010 on the Century 250 amp AC/DC transformer machine.
    The 6010 is the Lincoln grey rod.
    No VRD on my machine.
    I'm not sure about input voltage, my plugin is one of those four prong "explodable" types.
    I had initially dismissed too low OCV, since I can maintain some pretty long arc lengths with other rods, but maybe I'm mistaken.
    I'll be back to welding on Friday, I'll play around with the 6010 a little more. I did find that welding with it was much easier of I stick the rod and let it heat up for 10 seconds before striking the arc.
    I hope not !!!
    I think you mean "convertible" similar to a clothes dryer, or Oven plug , flat blades having several voltage/amperage configurations. If residential, then most likely 230vac, probably not the input being the problem.
    Its a very good chance its the welder itself, it just doesn't have the arc for it. No adjustments beyond Amps.

    Regards
    Last edited by albrightree; 10-07-2021 at 04:59 PM.
    Airco 250 ac/dc Heliwelder Square wave
    Miller Synchrowave 180 sd
    Miller Econo Twin HF
    Lincoln 210 MP
    Dayton 225 ac/dc
    Victor torches
    Snap-On YA-212
    Lotos Cut60D
    Primeweld 225 ac/dc
    Primeweld mig180
    Miller AEAD-200

  10. Likes 52 Ford, John Baptist liked this post
  11. #9
    Join Date
    Jun 2012
    Location
    CT
    Posts
    6,501
    Post Thanks / Like

    Re: Issue with 6010 arc

    Probably the OCV is too low. Those welders have a high range and a low range on AC, which actually does affect the OCV (higher OCV in low range). I'd bet a dollar that the DC side of that welder is connected to the high range of the transformer. You could figure it out pretty quick with an AC/DC voltage meter. But honestly for that machine, just get some of the Hobart 6011 at Tractor Supply and go to town. Those Hobart 6011's are really nice:

    Name:  6011.jpg
Views: 2139
Size:  286.1 KB
    Miller Multimatic 255

  12. Likes John Baptist, kjemison1966 liked this post
  13. #10
    Join Date
    Jun 2012
    Location
    Laredo + Midland/Odessa
    Posts
    7,132
    Post Thanks / Like

    Re: Issue with 6010 arc

    Quote Originally Posted by Carbon-Arc View Post
    I did find that welding with it was much easier of I stick the rod and let it heat up for 10 seconds before striking the arc.
    Don't let that fool you though. A machine that is capable of running 6010, sticking the rod is not necessary. Just the fact that you have to bury the rod to keep it lit really tells the whole story. It really does.
    1st on WeldingWeb to have a scrolling sig!



  14. #11
    Join Date
    Jun 2021
    Posts
    132
    Post Thanks / Like

    Re: Issue with 6010 arc

    albrightree- I do mean explodable. It's a specific type of connector at the college, not a regular home plug-in. There is no adjustment besides amperage on my machine.
    I'll try the 6011 on DC, if it is also hard to run, I'll chock it up to too low OCV.
    IWW member
    Century: 250 amp AC/DC, 295 amp AC, High Frequency Box
    Victor, Harris, and Oxweld Oxy-Acetylene Equipment.

  15. #12
    Join Date
    Jul 2008
    Posts
    3,312
    Post Thanks / Like

    Re: Issue with 6010 arc

    It's interesting and kinda surprising to me that it's the OCV in inerters that causes trouble with 6010, because on my engine drive welder, when I'm burning 6010 and want a lot of dig / "arc force" I turn the "fine" adjustment way down (this varies the OCV and also lets you use multiple "coarse" ranges for the same given amperage) ... so when I'm putting in a root with 6010, and want lots of dig, I set the range tap at one of the upper ranges, and set the "fine" adjustment way down around 10% ... which gives an OCV of probably less than 65VDC (by using the fine adjustment, I can get OCV from 58VDC at the bottom to 88VDC at the top)... this low OCV makes the 6010 very "sticky" at arc startup, but once the arc is lit, you can gouge holes in your material like an oxylance...

    I guess the electronics and everything else are different, giving different behavior on an engine drive versus an inerter...anyway, not to go TOO far OT...

  16. #13
    Join Date
    Jul 2021
    Posts
    338
    Post Thanks / Like

    Re: Issue with 6010 arc

    Quote Originally Posted by Carbon-Arc View Post
    To answer all questions:
    I did find that welding with it was much easier of I stick the rod and let it heat up for 10 seconds before striking the arc.

    I've seen this issue before with trying to run 6010 on under powered machines. I would have to drag the rod across the steel to get the tip of the rod hot enough to hold an arch. Not enough amps to start up and run.

    It honestly just sounds like it needs more amps. What happens when you start to crank the amps up?
    Airco Auto-Pak 130

    Forney 235AC/DC

    Miller Econo Tig

  17. #14
    Join Date
    Jun 2021
    Posts
    132
    Post Thanks / Like

    Re: Issue with 6010 arc

    When I turn the amps up, not much happens. With 1/8in rod, 6010 will have an equally hard time at 100 amps, or at 160 amps.
    Meanwhile the 6011 will run fine on DC as well.
    IWW member
    Century: 250 amp AC/DC, 295 amp AC, High Frequency Box
    Victor, Harris, and Oxweld Oxy-Acetylene Equipment.

  18. #15
    Join Date
    Oct 2014
    Posts
    5,270
    Post Thanks / Like

    Re: Issue with 6010 arc

    It's just the machine. If it was an Idealarc 250 or Dialarc 250 it would run 6010 pretty good but these machines are quite an upgrade from the Century. If it runs 6011, use that.

  19. Likes 12V71 liked this post
  20. #16
    Join Date
    May 2014
    Location
    Central Wa. state
    Posts
    8,196
    Post Thanks / Like

    Re: Issue with 6010 arc

    Quote Originally Posted by Carbon-Arc View Post
    When I turn the amps up, not much happens. With 1/8in rod, 6010 will have an equally hard time at 100 amps, or at 160 amps.
    Meanwhile the 6011 will run fine on DC as well.
    You may have the OCV, but its not holding up arc volts. Most of those cheaper machines wont. 6011 has added arc stabilizers to maintain the arc on A/C and that helps with low volt D/C welding. Stick with some good 6011, 6010 is no better if your machine wont run it.

  21. #17
    Join Date
    Feb 2014
    Location
    VIRGINIA,MN
    Posts
    380
    Post Thanks / Like

    Re: Issue with 6010 arc

    Try for kicks and giggles, find some red 6010. I had a AC only stick machine that would not run 7018 or gray 5p+ 6010. But give it some red 6010 and it welded fine. Can't explain it, it just worked. Other wise, as others have said, 6011 is very nice!

  22. Likes Carbon-Arc liked this post
  23. #18
    Join Date
    Mar 2018
    Location
    Clovis California
    Posts
    9,896
    Post Thanks / Like

    Re: Issue with 6010 arc

    I agree 👍
    I said same thing in one first posts.

    Dave

    Quote Originally Posted by Welder Dave View Post
    It's just the machine. If it was an Idealarc 250 or Dialarc 250 it would run 6010 pretty good but these machines are quite an upgrade from the Century. If it runs 6011, use that.

  24. Likes Plugg liked this post
  25. #19
    Join Date
    Apr 2021
    Location
    Adelaide, South Australia
    Posts
    431
    Post Thanks / Like

    Re: Issue with 6010 arc

    I've never tried 6010 but as it features so much I thought I'd give it a go. Turns out that's easier said than done. Not a common rod in Australia and there are very few stockists so I can only order in bulk.

    I ordered a 10lb packet of Forney 1/8" E6010 from the US. I don't know if that is any good but I'll find out in a few months. Unfortunately the USPS has suspended shipments to Australia because two of the 10 international airports are disrupted due to COVID-19. Lack of international flights is an ongoing problem as most of the packages come on passenger flights.

    Hopefully the flux is still attached to the rods when it gets here.

    Jack

  26. #20
    Join Date
    Mar 2018
    Location
    Clovis California
    Posts
    9,896
    Post Thanks / Like

    Re: Issue with 6010 arc

    I was told a long time ago that single phase welder has poor DC for some type welding. Single phase has 120 hz. A three phase and a true DC welder dose not have the odd cycle.

    A few single phase welder will use a bank of capacitors.
    I know when I use a DC welder generator it is lot smooth arc.
    This maybe your problem

    Dave

    Quote Originally Posted by Carbon-Arc View Post
    Welding with 6010+ on either straight or reverse polarity is pretty difficult on my machine. The arc likes to extinguish frequently, and to maintain the arc as best as possible, I'm finding that I have to bury the tip of the rod in the molten flux puddle.
    6011 will run completely fine at the same amperage (on AC).
    Is this some inherent fault of my machine, or do I need to adjust something?

+ Reply to Thread

Quick Reply Quick Reply

Register Now

Please enter the name by which you would like to log-in and be known on this site.

Please enter a password for your user account. Note that passwords are case-sensitive.

Please enter a valid email address for yourself.

A) Welding/Fabrication Shop
B) Plant/Production Line
C) Infrastructure/Construction/Repair or Maintenance/Field Work
D) Distributor of Welding Supplies or Gases
E) College/School/University
F) Work Out of Home

A) Corporate Executive/Management
B) Operations Management
C) Engineering Management
D) Educator/Student
E) Retired
F) Hobbyist

Log-in

Posting Permissions

  • You may post new threads
  • You may post replies
  • You may not post attachments
  • You may not edit your posts
  •  
Page generated in 1,713,292,970.48277 seconds with 20 queries